A kind of nano-aggregate aluminum oxide for polishing and its preparation method and application

Nano-grominated alumina was prepared by spray granulation method and used for silicon carbide wafer polishing, which solved the problems of low efficiency and high roughness of traditional polishing liquids, and achieved high efficiency removal rate and low roughness polishing effect.

CN116023861BActive Publication Date: 2024-11-29HUANGPU INST OF MATERIALS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211590024.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-12
Publication Date
2024-11-29
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

Traditional polishing liquids are inefficient in silicon carbide wafer polishing process, easily cause scratches and high roughness, and nano-gross alumina is less used in this field.

Method used

Nano-grominated alumina is prepared by spray granulation method. By dispersing nano-alumina, water reducing agent, ceramic binding agent and polyether ether ketone in water, it forms a composite abrasive embryo, and mixes it with sodium chloride and sintered at high temperature. , nano-gross alumina was prepared, which was used to prepare a polishing liquid to improve the polishing effect of the silicon carbide wafer.

Benefits of technology

The polishing effect of ensuring high removal rate while maintaining low roughness is achieved, avoiding scratches, and destroying the chemical bonds on the surface of silicon carbide through strong oxidants, improving the removal rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003993755000000011
    Figure HDA0003993755000000011
  • Figure HDA0003993755000000012
    Figure HDA0003993755000000012
  • Figure HDA0003993755000000021
    Figure HDA0003993755000000021
Patent Text Reader

Abstract

The present invention belongs to the technical field of nano-abrasive preparation, and is a kind of nano-agglomerated aluminum oxide for polishing and its preparation method and application, comprising the following steps: (1) dispersing nano-alumina, a water reducing agent, a ceramic binder and polyetheretherketone in water, mixing them evenly by ultrasonic stirring to obtain a mixed slurry, and then spraying granulation to obtain a composite abrasive embryo; (2) mixing the composite abrasive embryo with sodium chloride evenly, and then sintering at high temperature; (3) washing and drying the mixture after sintering in step (2) to obtain nano-agglomerated aluminum oxide. The present invention uses nano-agglomerated aluminum oxide as an abrasive, and synthesizes large particles by small-particle spray granulation. Compared with traditional α-alumina, while maintaining high hardness and high cutting force, the original grain size is small and the morphology is spherical, which can simultaneously ensure better roughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano-abrasive preparation, and relates to a method for preparing nano-agglomerated aluminum oxide and its polishing application. Background Art

[0002] Silicon carbide (SiC) is an ideal semiconductor material for making high-temperature, high-frequency and high-power power electronic devices. It is one of the main representatives of the third-generation semiconductors. Compared with traditional silicon-based products, the devices made of it can provide core guarantees for the upgrade of power electronic products, such as new energy vehicles, charging piles, photovoltaic power generation and other fields. With the rapid development of the semiconductor industry, the size of electronic devices is getting smaller and smaller, and the requirements for the wafer surface are getting higher and higher, requiring the surface roughness of the wafer to reach the nanometer level.

[0003] Traditional planarization technology can only achieve local planarization, while chemical mechanical polishing (CMP) technology can not only achieve global planarization, but also outperform traditional planarization technology in processing performance and speed. For CMP of silicon carbide wafers, polishing liquid is a very important consumable. In the prior art, due to the high hardness of silicon carbide wafers, traditional polishing liquid has low processing efficiency, increased production costs, and easy scratches on the polished surface.

[0004] At present, α-alumina is widely used in grinding and polishing consumables due to its high hardness, but it is rarely used in silicon carbide polishing liquid, and there is no limited morphology, mostly irregular morphology. This leads to the fact that when polishing silicon carbide, although the removal rate is high when the particle size is large, it is easy to cause scratches, resulting in greater roughness; the roughness is small when the particle size is small, but the removal rate is also low. Nano-agglomerated alumina is formed by the agglomeration of small-particle nano-alumina to form large-particle alumina, which can maintain a low roughness while ensuring a high removal rate. However, there are currently few reports on the application of nano-agglomerated alumina in silicon carbide polishing liquid. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a nano-aggregate aluminum oxide and a preparation method and polishing application thereof.

[0006] The technical solution of the present invention is as follows:

[0007] A method for preparing nano-aggregate aluminum oxide for polishing comprises the following steps:

[0008] (1) dispersing nano-alumina, a water reducing agent, a ceramic binder and polyetheretherketone in water, mixing them uniformly by ultrasonic stirring to obtain a mixed slurry, and then spray granulating them to obtain a composite abrasive embryo;

[0009] (2) mixing the composite abrasive embryo and sodium chloride uniformly, and then sintering at high temperature;

[0010] (3) The mixture after sintering in step (2) is washed with water and dried to obtain nano-aggregate aluminum oxide.

[0011] Preferably, the spray granulation in step (1) adopts a spray dryer with a rotation speed of 30000±20000rpm, a spray granulation temperature of 300±100°C, and a time of 6±3h.

[0012] Preferably, in step (2), the mass ratio of the composite abrasive embryo to sodium chloride is 1:1-5:1; the high-temperature sintering temperature is 250-500° C., and the sintering time is 1-5 h.

[0013] Preferably, in step (2), the mass ratio of the composite abrasive embryo to sodium chloride is 3:1; the high-temperature sintering temperature is 350° C., and the sintering time is 3 hours.

[0014] Preferably, the proportion of the mixed slurry in step (1) is: 10-30% nano-alumina powder, 10-30% polyetheretherketone, 1-10% water reducer, 10-30% ceramic binder, and 20-60% water, by mass; the water reducer is sodium lignin sulfonate, and the ceramic binder is low-temperature melting glass powder. When the amount of alumina increases, the amount of water reducer decreases; the amount of ceramic binder and polyetheretherketone can adjust the particle size of the aggregate.

[0015] Preferably, the ratio of the mixed slurry in step (1) is: 15-25% nano-alumina powder, 15-25% polyetheretherketone, 2-5% water reducer, 15-25% ceramic binder, and 30-50% water; the purity of the nano-alumina is ≥99.9%, the particle size of the nano-alumina is 10-200nm, and the particle size of the polyetheretherketone is 10-200nm.

[0016] Preferably, in step (1), the ultrasonic power is 800-1500 W, and the time is 30±20 min; in step (3), the drying temperature is 120±30° C.; and the drying time is 5±3 h.

[0017] A nano-agglomerated aluminum oxide polishing liquid comprises the following components by weight percentage:

[0018] 1-10% of nano-agglomerated aluminum oxide, 0.05%-5% of a surfactant, 0.2-5% of an oxidant, 0.02%-2% of an acidic regulator, 0.05%-5% of a complexing agent, and the balance being an aqueous medium; the particle size of the nano-agglomerated aluminum oxide is 0.5-5um.

[0019] The preparation method of the polishing liquid comprises the following steps:

[0020] (1) adding a surfactant, a complexing agent, and an oxidant into water, stirring and dissolving them to prepare a premixed solution;

[0021] (2) adding an acidic regulator and alumina powder to water and stirring evenly; pouring the premixed solution of step (1) into the mixed solution while stirring, and finally adjusting the pH value to 2-4 to obtain a nano-alumina polishing solution.

[0022] The surfactant is one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, dodecylbenzene sulfonic acid, alkylphenol polyoxyethylene ether, and hexadecyltrimethylammonium chloride.

[0023] The oxidant is one or more of potassium permanganate, potassium ferrate, potassium dichromate, sodium persulfate, hydrogen peroxide, chromic anhydride, and ferric nitrate.

[0024] The acidic regulator is one or more of citric acid, formic acid, acetic acid, oxalic acid, nitric acid, hydrochloric acid, sulfuric acid, glycine, and phosphoric acid.

[0025] The complexing agent is one or more of triammonium citrate, ethylenediaminetetraacetic acid and its salts, hydroxyethylidene diphosphonic acid and its salts, ascorbic acid, and oxalic acid.

[0026] The nano-agglomerated aluminum oxide polishing liquid is applied to polishing silicon carbide wafers.

[0027] The principle of the present invention is as follows: Nano-agglomerated alumina is prepared by spray granulation. During the polishing process, the alumina aggregates are spherical and are not easily scratched. The polishing process will peel off the original small-particle nano-alumina to repair the roughness. The large particles themselves play a physical cutting role, so while ensuring a high removal rate, it can also have a better roughness.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) The present invention adds sodium chloride to the alumina composite abrasive blank. The sodium chloride has high temperature resistance and does not chemically react with the alumina composite abrasive blank. It plays a role of separation when the composite abrasive blank is sintered to increase its strength, thereby avoiding adhesion between particles of the composite abrasive blank during the sintering process.

[0030] (2) The present invention uses nano-agglomerated aluminum oxide as an abrasive and synthesizes large particles by spray granulation of small particles. Compared with traditional α-alumina, while maintaining high hardness and high cutting force, the original grain size is small and the morphology is spherical, which can also ensure better roughness.

[0031] (3) The present invention uses a strong oxidant to destroy the chemical bonds between silicon carbides, making the surface of silicon carbide more easily oxidized to form a loose oxide layer, which is then ground and peeled off by aluminum oxide, thereby improving the removal rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1This is the SEM morphology of the nano-aggregate aluminum oxide in Example 1.

[0033] Figure 2 This is a partially enlarged view of the SEM morphology of the nano-aggregate aluminum oxide in Example 2.

[0034] Figure 3 This is the SEM morphology of the nano-aggregate aluminum oxide in Example 2.

[0035] Figure 4 This is an AFM image of the surface roughness of the silicon carbide wafer after polishing in Example 1, with a roughness of 0.1143 nm.

[0036] Figure 5 This is the SEM morphology of ordinary α-nano alumina in Comparative Example 1.

[0037] Figure 6 This is the SEM morphology of the nano-aggregate aluminum oxide in Example 5. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below in conjunction with specific embodiments, but the embodiments of the present invention are not limited thereto. For process parameters not particularly noted, conventional techniques may be used.

[0039] The nano-alumina used in this experiment is VK-AL03 from Xuancheng Jingrui New Materials Co., Ltd.; the ordinary α-nano-alumina is C500 from Dalian International Trade Agency; the ceramic binder is the low-temperature melting glass powder from Foshan Jinggu Materials Technology Co., Ltd.; the other reagents are all commercially available products from Xilong.

[0040] Example 1

[0041] Preparation of nano-aggregate alumina:

[0042] ① Disperse 250g 10nm nano-alumina, 20g sodium lignin sulfonate, 200g low-temperature melting glass powder and 200g 10nm polyetheretherketone in 330g water, stir and mix evenly by ultrasonic for 30min to prepare a mixed slurry;

[0043] ② The mixed slurry prepared in step ① was sprayed and granulated by a spray dryer at a temperature of 300° C., a rotation speed of 30,000 rpm, and a time of 6 h to obtain a composite abrasive embryo;

[0044] ③ The composite abrasive blank prepared in step ② was mixed evenly with sodium chloride in a mass ratio of 3:1, and then placed in a muffle furnace and dried at 350° C. for 3 h to obtain a mixture of composite abrasive and sodium chloride;

[0045] ④ Place the composite abrasive prepared in step ③ and the mixture of sodium chloride in water, dissolve the sodium chloride in the water, rinse the composite abrasive, and dry it at 120° C. for 5 hours to obtain a composite abrasive of mixed particle size;

[0046] ⑤ The composite abrasive of mixed particle size obtained in step ④ is sieved with a sieve to obtain nano-agglomerated aluminum oxide with a particle size of 2-3 um.

[0047] Preparation of nano-aggregate alumina polishing liquid:

[0048] (1) Add 5 g of hexadecyltrimethylammonium chloride, 5 g of oxalic acid, and 50 g of potassium permanganate to 440 g of water, stir and dissolve to prepare a premix;

[0049] (2) Add 5 g of nitric acid and 100 g of nano-aggregate alumina into 395 g of water and stir evenly;

[0050] (3) Pour the premixed solution of step (1) into the mixed solution of step (2) while stirring, and finally adjust the pH value to 3 to obtain a polishing solution for silicon carbide wafers.

[0051] Example 2

[0052] Preparation of nano-aggregate alumina:

[0053] ① Disperse 200g 20nm nano-alumina, 30g sodium lignin sulfonate, 150g low-temperature melting glass powder and 200g 20nm polyetheretherketone in 420g water, stir and mix evenly by ultrasonic for 30min to prepare a mixed slurry;

[0054] ② The mixed slurry prepared in step ① was sprayed and granulated by a spray dryer at a temperature of 300° C., a rotation speed of 30,000 rpm, and a time of 6 h to obtain a composite abrasive embryo;

[0055] ③ The composite abrasive blank prepared in step ② was mixed evenly with sodium chloride in a mass ratio of 3:1, and then placed in a muffle furnace and dried at 350° C. for 3 h to obtain a mixture of composite abrasive and sodium chloride;

[0056] ④ Place the composite abrasive prepared in step ③ and the mixture of sodium chloride in water, dissolve the sodium chloride in the water, rinse the composite abrasive, and dry it at 120° C. for 5 hours to obtain a composite abrasive of mixed particle size;

[0057] ⑤ The composite abrasive of mixed particle size obtained in step ④ is sieved with a sieve to obtain nano-agglomerated aluminum oxide with a particle size of 3-4 um.

[0058] Preparation of nano-aggregate alumina polishing liquid:

[0059] (1) 10 g of dodecylbenzene sulfonic acid, 10 g of ascorbic acid, 40 g of hydrogen peroxide and 5 g of ferric nitrate were added to 435 g of water respectively, stirred and dissolved to prepare a premix;

[0060] (2) Add 10 g of nitric acid and 90 g of nano-aggregate alumina into 400 g of water and stir evenly;

[0061] (3) Pour the premixed solution of step (1) into the mixed solution of step (2) while stirring, and finally adjust the pH value to 3 to obtain a polishing solution for silicon carbide wafers.

[0062] Example 3

[0063] Preparation of nano-aggregate alumina:

[0064] ① Disperse 150g of 10nm nano-alumina, 50g of sodium lignin sulfonate, 150g of low-temperature melting glass powder and 200g of polyetheretherketone in 450g of water, stir and mix evenly by ultrasonic for 30min to prepare a mixed slurry;

[0065] ② The mixed slurry prepared in step ① was sprayed and granulated by a spray dryer at a temperature of 300° C., a rotation speed of 30,000 rpm, and a time of 6 h to obtain a composite abrasive embryo;

[0066] ③ The composite abrasive blank prepared in step ② was mixed evenly with sodium chloride in a mass ratio of 3:1, and then placed in a muffle furnace and dried at 350° C. for 3 h to obtain a mixture of composite abrasive and sodium chloride;

[0067] ④ Place the composite abrasive prepared in step ③ and the mixture of sodium chloride in water, dissolve the sodium chloride in the water, rinse the composite abrasive, and dry it at 120° C. for 5 hours to obtain a composite abrasive of mixed particle size;

[0068] ⑤ The composite abrasive of mixed particle size obtained in step ④ is sieved with a sieve to obtain nano-agglomerated aluminum oxide with a particle size of 0.5-1 um.

[0069] Preparation of nano-aggregate alumina polishing liquid:

[0070] (1) Add 1 g of sodium dodecyl sulfate, 9 g of triammonium citrate, and 10 g of potassium ferrate to 480 g of water, stir and dissolve to prepare a premix;

[0071] (2) Add 20 g of phosphoric acid and 80 g of nano-granular alumina into 400 g of water and stir evenly;

[0072] (3) Pour the premixed solution of step (1) into the mixed solution of step (2) while stirring, and finally adjust the pH value to 2 to obtain a polishing solution for silicon carbide wafers.

[0073] Example 4

[0074] Preparation of nano-aggregate alumina:

[0075] ① Disperse 180g of 20nm nano-alumina, 50g of sodium lignin sulfonate, 180g of low-temperature melting glass powder and 180g of polyetheretherketone in 410g of water, stir and mix them evenly by ultrasonic for 30min to prepare a mixed slurry;

[0076] ② The mixed slurry prepared in step ① was sprayed and granulated by a spray dryer at a temperature of 300° C., a rotation speed of 30,000 rpm, and a time of 6 h to obtain a composite abrasive embryo;

[0077] ③ The composite abrasive blank prepared in step ② was mixed evenly with sodium chloride in a mass ratio of 3:1, and then placed in a muffle furnace and dried at 350° C. for 3 h to obtain a mixture of composite abrasive and sodium chloride;

[0078] ④ Place the composite abrasive prepared in step ③ and the mixture of sodium chloride in water, dissolve the sodium chloride in the water, rinse the composite abrasive, and dry it at 120° C. for 5 hours to obtain a composite abrasive of mixed particle size;

[0079] ⑤ The composite abrasive of mixed particle size obtained in step ④ is sieved with a sieve to obtain nano-agglomerated aluminum oxide with a particle size of 1-2 um.

[0080] Preparation of nano-aggregate alumina polishing liquid:

[0081] (1) Add 1 g of hexadecyltrimethylammonium chloride, 1 g of oxalic acid, and 8 g of potassium permanganate to 490 g of water, stir and dissolve to prepare a premix;

[0082] (2) Add 5 g of hydrochloric acid and 75 g of nano-aggregate alumina to 420 g of water and stir evenly;

[0083] (3) Pour the premixed solution of step (1) into the mixed solution of step (2) while stirring, and finally adjust the pH value to 4 to obtain a polishing solution for silicon carbide wafers.

[0084] Example 5

[0085] Preparation of nano-aggregate alumina:

[0086] ① Disperse 250g of 50nm nano-alumina, 20g of sodium lignin sulfonate, 200g of low-temperature melting glass powder and 200g of polyetheretherketone in 330g of water, stir and mix them evenly by ultrasonic for 30min to prepare a mixed slurry;

[0087] ② The mixed slurry prepared in step ① was sprayed and granulated by a spray dryer at a temperature of 300° C., a rotation speed of 30,000 rpm, and a time of 6 h to obtain a composite abrasive embryo;

[0088] ③ The composite abrasive blank prepared in step ② was mixed evenly with sodium chloride in a mass ratio of 3:1, and then placed in a muffle furnace and dried at 350° C. for 3 h to obtain a mixture of composite abrasive and sodium chloride;

[0089] ④ Place the composite abrasive prepared in step ③ and the mixture of sodium chloride in water, dissolve the sodium chloride in the water, rinse the composite abrasive, and dry it at 120° C. for 5 hours to obtain a composite abrasive of mixed particle size;

[0090] ⑤ The composite abrasive of mixed particle size obtained in step ④ is sieved with a sieve to obtain nano-agglomerated aluminum oxide with a particle size of 4-5 um.

[0091] Preparation of nano-aggregate alumina polishing liquid:

[0092] (1) Add 3 g of alkylphenol polyoxyethylene ether, 2 g of tetrasodium ethylenediaminetetraacetate, and 35 g of potassium dichromate to 460 g of water, stir and dissolve to prepare a premix;

[0093] (2) Add 10 g of sulfuric acid and 70 g of nano-aggregate alumina to 420 g of water and stir evenly;

[0094] (3) Pour the premixed solution of step (1) into the mixed solution of step (2) while stirring, and finally adjust the pH value to 3 to obtain a polishing solution for silicon carbide wafers.

[0095] Comparative Example 1

[0096] The difference between the present invention and Example 1 is that: (using ordinary α-nano alumina)

[0097] (1) Add 5 g of hexadecyltrimethylammonium chloride, 5 g of oxalic acid, and 50 g of potassium permanganate to 440 g of water, stir and dissolve to prepare a premix;

[0098] (2) Add 5 g of nitric acid and 100 g of ordinary α-nano alumina to 395 g of water and stir evenly;

[0099] (3) Pour the premixed solution of step (1) into the mixed solution of step (2) while stirring, and finally adjust the pH value to 3 to obtain a polishing solution for silicon carbide wafers.

[0100] Comparative Example 2

[0101] The difference between the present invention and Example 1 is that: (no oxidant is used)

[0102] ① Disperse 250g of nano-alumina, 20g of sodium lignin sulfonate, 200g of ceramic binder and 200g of polyetheretherketone in 330g of water, stir and mix them evenly by ultrasonic for 30min to prepare a mixed slurry;

[0103] ② The mixed slurry prepared in step ① was sprayed and granulated by a spray dryer at a temperature of 300° C., a rotation speed of 30,000 rpm, and a time of 6 h to obtain a composite abrasive embryo;

[0104] ③ The composite abrasive blank prepared in step ② was mixed evenly with sodium chloride in a mass ratio of 3:1, and then placed in a muffle furnace and dried at 350° C. for 3 h to obtain a mixture of composite abrasive and sodium chloride;

[0105] ④ Place the composite abrasive prepared in step ③ and the mixture of sodium chloride in water, dissolve the sodium chloride in the water, rinse the composite abrasive, and dry it at 120° C. for 5 hours to obtain a composite abrasive of mixed particle size;

[0106] ⑤ The composite abrasive of mixed particle size obtained in step ④ is sieved with a sieve to obtain 2-3um nano-aggregate aluminum oxide.

[0107] Preparation of nano-aggregate alumina polishing liquid:

[0108] (1) Add 5 g of hexadecyltrimethylammonium chloride and 5 g of oxalic acid to 490 g of water, stir and dissolve to prepare a premix;

[0109] (2) Add 5 g of nitric acid and 100 g of nano-aggregate alumina into 395 g of water and stir evenly;

[0110] (3) Pour the premixed solution of step (1) into the mixed solution of step (2) while stirring, and finally adjust the pH value to 3 to obtain a polishing solution for silicon carbide wafers.

[0111] The above embodiments and comparative examples were formulated into polishing liquids, and silicon carbide wafers were polished under the same polishing conditions, and the polishing parameters were as follows: a Chuangji 36DAW polishing machine, a DuPont SUBA800 polishing pad, a downward pressure of 4 psi, a turntable speed / polishing head speed = 93 / 108 rpm, a polishing time of 600 s, and a chemical mechanical polishing slurry flow rate of 100 mL / min.

[0112] Table 1

[0113] Serial number Removal rate (nm / min) Roughness(nm) Scratches Example 1 178 0.1143 none Example 2 137 0.1525 none Example 3 103 0.0612 none Example 4 106 0.0725 none Example 5 194 0.1798 none Comparative Example 1 71 0.5624 Small amount Comparative Example 2 64 0.2487 none

[0114] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A silicon carbide polishing liquid, characterized in that: Nano-aggregate aluminum oxide is used as an abrasive, and the preparation method of the nano-aggregate aluminum oxide comprises the following steps: (1) dispersing nano-alumina, a water reducing agent, a ceramic binder and polyetheretherketone in water, mixing them uniformly by ultrasonic stirring to obtain a mixed slurry, and then spray granulating them to obtain a composite abrasive embryo; the water reducing agent is sodium lignin sulfonate, and the ceramic binder is low-temperature melting glass powder; (2) Evenly mixing the composite abrasive embryo and sodium chloride, and then sintering at high temperature; (3) The mixture after sintering in step (2) is washed with water and dried to obtain nano-aggregate alumina.

2. The polishing liquid according to claim 1, characterized in that The spray granulation in step (1) adopts a spray dryer with a rotation speed of 30000±20000rpm, a spray granulation temperature of 300±100°C, and a time of 6±3h.

3. The polishing liquid according to claim 1, characterized in that In step (2), the mass ratio of the composite abrasive embryo to sodium chloride is 1:1-5:1; the high-temperature sintering temperature is 250-500° C., and the sintering time is 1-5 hours.

4. The polishing liquid according to claim 3, characterized in that The proportion of the mixed slurry in step (1) is, by weight, 10-30% nano-alumina, 10-30% polyetheretherketone, 1-10% water reducer, 10-30% ceramic binder, and 20-60% water.

5. The polishing liquid according to claim 4, characterized in that: Step (1) The mixing ratio of the mixed slurry is: 15-25% nano-alumina, 15-25% polyetheretherketone, 2-5% water reducer, 15-25% ceramic binder, and 30-50% water; the particle size of the nano-alumina is 10-200nm, and the particle size of the polyetheretherketone is 10-200nm; In step (2), the mass ratio of the composite abrasive embryo to sodium chloride is 3:1; the high-temperature sintering temperature is 350° C. and the sintering time is 3 h.

6. The polishing liquid according to claim 4, characterized in that In step (1), the ultrasonic power is 800-1500 W and the drying time is 30±20 min. In step (3), the drying temperature is 120±30° C. and the drying time is 5±3 h.

7. The polishing liquid according to any one of claims 1 to 6, characterized in that In terms of weight percentage, it includes the following components: 1-10% of nano-agglomerated aluminum oxide, 0.05%-5% of a surfactant, 0.2-5% of an oxidant, 0.02%-2% of an acidic regulator, 0.05%-5% of a complexing agent, and the balance being an aqueous medium; the particle size of the nano-agglomerated aluminum oxide is 0.5-5 μm.

8. The polishing liquid according to claim 7, characterized in that: The preparation method of the polishing liquid comprises the following steps: (1) Add surfactant, complexing agent and oxidant into water, stir and dissolve them to prepare a premixed solution; (2) adding an acidic regulator and nano-aggregate alumina into water and stirring evenly; pouring the premixed solution of step (1) into the mixed solution while stirring, and finally adjusting the pH value to 2-4 to obtain a polishing solution; The surfactant is one or more of sodium dodecyl sulfate, dodecylbenzenesulfonic acid and its sodium salt, alkylphenol polyoxyethylene ether, and hexadecyltrimethylammonium chloride; The oxidant is one or more of potassium permanganate, potassium ferrate, potassium dichromate, sodium persulfate, hydrogen peroxide, chromic anhydride, and ferric nitrate; The acidic regulator is one or more of citric acid, formic acid, acetic acid, oxalic acid, nitric acid, hydrochloric acid, sulfuric acid, glycine, and phosphoric acid; The complexing agent is one or more of triammonium citrate, ethylenediaminetetraacetic acid and its salts, hydroxyethylidene diphosphonic acid and its salts, ascorbic acid, and oxalic acid.

9. The polishing liquid according to any one of claims 1 to 8 is used for polishing silicon carbide wafers.

Citation Information

Patent Citations

  • Diamond composite abrasive material for grinding and polishing and preparation method thereof

    CN114032068A

  • Nanometer aluminum oxide abrasive particle, preparation method, application and silicon carbide polishing solution containing abrasive particle

    CN114940886A