A nickel-cobalt-manganese oxysulfide electrode material and preparation method thereof
Through the design and preparation of nickel-cobalt-manganese oxysulfide electrode materials, the ternary metal oxalic acid compound and carbon doping technology is used to solve the problem of insufficient performance of supercapacitor electrode materials in the existing technology, and high energy density, power density and The improvement of cycle stability is suitable for the preparation of high-performance electrode materials.
Patent Information
- Application Number
- CN202310109825.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-14
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-02-14
AI Technical Summary
While the existing supercapacitor electrode materials improve energy density and power density, it is difficult to improve cycle performance and stability at the same time, and there is insufficient exploration of material design and synthesis methods.
Using nickel-cobalt-manganese oxysulfide electrode material, ternary metal organic frame material is prepared by stable structure ternary metal oxalic acid compound as a precursor, and through carbon doping treatment, the composition and morphological structure of the material are regulated, and multi-metals are used. The synergistic effect of compounds significantly improves electrochemical properties.
Significantly improves the energy density and power density of supercapacitors, and improves the cyclic stability and electrochemical performance of the material. It is suitable for the preparation of high-performance electrode materials, has strong applicability, is suitable for mass production, and can be expanded to other metal oxalic acids. Preparation of compounds.
Smart Images

Figure CN116031077B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an electrode material for a supercapacitor, and in particular to a nickel-cobalt-manganese oxysulfide electrode material and a preparation method thereof. Background Art
[0002] Energy issues are one of the biggest challenges facing mankind in the 21st century. In order to meet the needs of human social progress and economic development, it is urgent to develop high-efficiency, low-cost, renewable, environmentally friendly clean energy and energy storage devices. As a power-type energy storage device, supercapacitors have the advantages of high power density, long cycle life, excellent rate performance, and fast charging and discharging. However, their low energy density greatly limits the development and application of supercapacitors. The energy density of supercapacitors can be effectively improved by designing high-performance electrode materials. Nickel-based metal compounds, as supercapacitor electrode materials, have always been valued by technicians due to their relatively high theoretical specific capacity.
[0003] Nickel cobalt sulfide (NCS) / graphene composites were successfully prepared by microwave method. The electrochemical test results show that at 0.5Ag -1 At this current density, the specific capacitance of the composite material is 710Fg -1 , and after 10,000 cycles, its specific capacitance retention rate is 75%. In addition, for the assembled supercapacitor (NCS / graphene / / ACASC), when the power density is 400Wkg -1 When the energy density is 30.29Whkg -1 . By rationally designing electrode materials and improving their specific capacitance, the energy density and power density of supercapacitors can be effectively improved, but their comprehensive performance such as cycle performance, energy density and power density is still difficult to meet application requirements. At present, the relevant materials reported in the relevant literature still have the problem of being difficult to simultaneously improve their specific capacitance, rate performance and cycle stability, and thus significantly improve the energy density and power density of supercapacitors, and there is a lack of exploration of material design and synthesis methods. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention creatively conceives a nickel-cobalt-manganese oxysulfide electrode material and a preparation method thereof, uses a ternary metal oxalate compound with a stable structure as a precursor, prepares a ternary metal organic framework material, effectively regulates the composition and morphology of the material, and further prepares a carbon-doped ternary metal oxysulfide composite electrode material, fully utilizing the synergistic effect between different metals in the multi-metal compound, significantly improving the electrochemical properties of the electrode material, and the constructed supercapacitor energy storage device also exhibits relatively ideal energy density and power density.
[0005] One of the technical solutions adopted to implement the present invention is: a nickel-cobalt-manganese oxysulfide electrode material, characterized in that, in the nickel-cobalt-manganese oxysulfide electrode material, the atomic ratio of nickel, cobalt and manganese is 2:0.5:0.3, and the nickel-cobalt-manganese oxysulfide electrode material is a micron-scale spherical structure, and the diameter of the micron-scale spherical structure is 2 to 9 um.
[0006] Furthermore, in the nickel-cobalt-manganese oxysulfide electrode material, the atomic ratio of nickel to sulfur is 1:1, 1:1.14 or 1:2.
[0007] The second technical solution adopted to realize the present invention is: a method for preparing a nickel-cobalt-manganese oxysulfide electrode material, characterized in that it comprises the following steps:
[0008] 1) Preparation of nickel-cobalt-manganese oxalate compound precursor:
[0009] 1.1) Dissolve Ni(NO3)2·6H2O and Co(NO3)2·6H2O in a molar ratio of 1:4 to 4:1, Ni(NO3)2·6H2O and C4H6MnO4·H2O in a molar ratio of 1:0.05 to 1:0.25, and Ni(NO3)2·6H2O and H2C2O4·2H2O in a molar ratio of 1:12 to 1:3 in 80 mL of ultrapure water and stir magnetically for 8 h at room temperature;
[0010] 1.2) Wash the product obtained in step 1.1) three times with ultrapure water;
[0011] 1.3) washing the product obtained in step 1.2) with anhydrous ethanol three times;
[0012] 1.4) placing the product obtained in step 1.3) in a forced air drying oven at 60° C. for 12 h to obtain a nickel-cobalt-manganese oxalate compound precursor;
[0013] 2) Preparation of nickel-cobalt-manganese oxysulfide electrode materials:
[0014] 2.1) Weigh 100 mg of the nickel-cobalt-manganese oxalate compound precursor obtained in step 1.4), evenly disperse it in 60 mL of ultrapure water, add 240-640 mg of NaOH, and stir at room temperature for 5-17 hours;
[0015] 2.2) washing the product obtained in step 2.1) with ultrapure water three times;
[0016] 2.3) washing the product obtained in step 2.2) with anhydrous ethanol three times;
[0017] 2.4) placing the product obtained in step 2.3) in a forced air drying oven at 60° C. for 12 h to obtain nickel-cobalt-manganese hydroxide;
[0018] 2.5) Weigh 20 mg of the nickel-cobalt-manganese hydroxide obtained in step 2.4), uniformly disperse it in a mixed solution of 3 mL of ultrapure water and 29 mL of N,N-dimethylformamide, and add 20 to 160 mg of 2,6-naphthalene dicarboxylic acid to obtain a dispersion;
[0019] 2.6) The dispersion obtained in step 2.5) was transferred into a reaction kettle, reacted at 130° C. for 6 hours, and then naturally cooled to 25° C.; 2.7) The product obtained in step 2.6) was washed three times with anhydrous ethanol;
[0020] 2.8) placing the product obtained in step 2.7) in a forced air drying oven at 60° C. for 12 h to obtain a nickel-cobalt-manganese-based metal organic framework material with a nanosheet self-assembled microsphere structure;
[0021] 2.9) Weigh the nanosheet self-assembled microsphere structure nickel-cobalt-manganese-based metal organic framework material obtained in step 2.8), evenly disperse it in 60 mL of ultrapure water, and add 80-140 mg of Na2S·9H2O;
[0022] 3.0) The dispersion obtained in step 2.9) was transferred into a reaction kettle, reacted at 90° C. for 6 h, and then naturally cooled to 25° C.; 3.1) The product obtained in step 3.0) was washed three times with ultrapure water;
[0023] 3.2) washing the product obtained in step 3.1) with anhydrous ethanol three times;
[0024] 3.3) The product obtained in step 3.2) was placed in a forced air drying oven and dried at 60° C. for 12 h to obtain a nickel-cobalt-manganese oxysulfide electrode material.
[0025] Furthermore, in the step 1.4), the nickel-cobalt-manganese oxalate compound precursor is a ternary metal oxalate compound with a block structure.
[0026] Furthermore, in the step 2.4), the nickel-cobalt-manganese hydroxide is a ternary metal hydroxide with a block structure.
[0027] Furthermore, in the steps 2.6) and 3.0), the reactor is a stainless steel reactor lined with polytetrafluoroethylene.
[0028] The beneficial effects of the nickel-cobalt-manganese oxysulfide electrode material and the preparation method thereof of the present invention are embodied in:
[0029] 1. A nickel-cobalt-manganese oxysulfide electrode material, which is a ternary metal oxide / sulfide composite material of nickel, cobalt and manganese, can make full use of the synergistic and complementary effect of multi-metal compounds to significantly improve the electrochemical performance of the material; at the same time, by preparing a nickel-cobalt-manganese-based metal organic framework intermediate, the composition and morphology of the material can be effectively regulated, carbon doping can be uniformly introduced into the composite material, and a relatively uniform lamellar structure can be formed, thereby increasing the specific surface area of the material, which is more conducive to the full contact between the electrolyte and the material, and thus significantly improving the energy storage performance of the material through composition and structural design;
[0030] 2. A method for preparing a nickel-cobalt-manganese oxysulfide electrode material, which is scientific and reasonable, has strong applicability and good effect, and is particularly suitable for preparing high-performance electrode materials. Under room temperature conditions, a simple chemical precipitation method is used to achieve the preparation of a nickel-cobalt-manganese oxalate compound precursor with adjustable composition and structure, and further prepares nickel-cobalt-manganese hydroxide and metal-organic framework materials, effectively regulating the composition and morphology of the materials, and using an anion exchange method to prepare a structurally stable carbon-doped nickel-cobalt-manganese oxysulfide composite electrode material;
[0031] 3. A method for preparing nickel-cobalt-manganese oxysulfide electrode materials is scientific and reasonable, safe and easy to operate, requires simple equipment, has low cost, and has controllable product morphology and structure. It is suitable for mass production of nickel-cobalt-manganese oxysulfide composite electrode materials. At the same time, this method can still be expanded to other monovalent, divalent and polyvalent metal oxalate compounds and their corresponding metal oxysulfides for controllable and large-scale preparation. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is a SEM image of the nickel-cobalt-manganese oxalate compound precursor prepared in the embodiment;
[0033] Figure 2 is a SEM image of nickel-cobalt-manganese hydroxide prepared in the embodiment;
[0034] Figure 3 is a SEM image of a nickel-cobalt-manganese-based metal organic framework prepared in an embodiment;
[0035] Figure 4 is a SEM image of nickel-cobalt-manganese oxysulfide prepared in the embodiment;
[0036] Figure 5 is an XRD pattern of a nickel-cobalt-manganese oxalate compound precursor prepared in an embodiment;
[0037] Figure 6 In the embodiment, the XRD pattern of the nickel-cobalt-manganese based metal organic framework is prepared;
[0038] Figure 7 In the examples, the XRD patterns of nickel cobalt manganese hydroxide and nickel cobalt manganese oxysulfide were prepared;
[0039] Figure 8 In the embodiment, the XPS graph of nickel cobalt manganese oxysulfide is prepared;
[0040] Fig. 9 In the embodiment, the prepared nickel-cobalt-manganese-oxysulfide electrode material has a -1 ~50mVs -1 Cyclic voltammogram at scan rate;
[0041] Fig.10 In the embodiment, the nickel-cobalt-manganese-oxysulfide electrode material prepared is 1Ag -1 ~20Ag -1 Constant current charge and discharge diagram under current density. DETAILED DESCRIPTION
[0042] The following is combined with Figures 1 to 10 The present invention is further described in detail with specific implementation modes, and the specific implementation modes described herein are only used to explain the present invention and are not used to limit the present invention.
[0043] A nickel-cobalt-manganese oxysulfide electrode material, wherein the atomic ratio of nickel, cobalt and manganese is 2:0.5:0.3, and the atomic ratio of nickel to sulfur is 1:1. The nickel-cobalt-manganese oxysulfide electrode material is a micron-scale spherical structure with a diameter of 3 to 7 um.
[0044] Embodiment 1:
[0045] The present embodiment provides a method for preparing a nickel-cobalt-manganese oxysulfide electrode material, including the following specific preparation steps:
[0046] 1) Preparation of nickel-cobalt-manganese oxalate compound precursor:
[0047] (1) Dissolve 1 mmol nickel nitrate (Ni(NO3)2·6H2O), 2 mmol cobalt nitrate (Co(NO3)2·6H2O), 0.1 mmol manganese acetate (C4H6MnO4·H2O) and 6 mmol oxalic acid (H2C2O4·2H2O) in 80 mL ultrapure water and stir magnetically at room temperature for 8 h;
[0048] (2) washing the product obtained in step (1) with ultrapure water three times;
[0049] (3) washing the product washed in step (2) with anhydrous ethanol three times;
[0050] (4) placing the product washed in step (2) and step (3) in a forced air drying oven and drying at 60° C. for 12 h to obtain a nickel-cobalt-manganese oxalate compound precursor, which is a block-structured ternary metal oxalate compound.
[0051] 2) Preparation of nickel-cobalt-manganese oxysulfide electrode materials:
[0052] (1) Weigh 100 mg of the nickel-cobalt-manganese oxalate compound precursor obtained in step 1), evenly disperse it in 60 mL of ultrapure water, add 640 mg of NaOH, and stir at room temperature for 5 h;
[0053] (2) washing the product obtained in step (1) with ultrapure water three times;
[0054] (3) washing the product washed in step (2) with anhydrous ethanol three times;
[0055] (4) placing the product washed in step (2) and step (3) in a forced air drying oven and drying at 60° C. for 12 h to obtain nickel-cobalt-manganese hydroxide, which is a ternary metal hydroxide with a block structure;
[0056] (5) Weigh 20 mg of nickel-cobalt-manganese hydroxide and evenly disperse it in a mixed solution of 3 mL of ultrapure water and 29 mL of N,N-dimethylformamide, and add 20 mg of 2,6-naphthalene dicarboxylic acid;
[0057] (6) The dispersion obtained in step (5) was transferred into a reaction vessel, reacted at 130° C. for 6 h, and then naturally cooled to room temperature;
[0058] (7) washing the product obtained in step (6) with anhydrous ethanol three times;
[0059] (8) placing the product washed in step (7) in a forced air drying oven and drying at 60° C. for 12 h to obtain a nickel-cobalt-manganese-based metal organic framework material with a nanosheet self-assembled microsphere structure;
[0060] (9) Weigh 20 mg of NiCoMn-based metal organic framework material, evenly disperse it in 60 mL of ultrapure water, and add 80 mg of Na2S·9H2O;
[0061] (10) The dispersion obtained in step (9) was transferred into a reaction vessel, reacted at 90° C. for 6 h, and then naturally cooled to room temperature;
[0062] (11) washing the product obtained in step (10) with ultrapure water three times;
[0063] (12) washing the product washed in step (11) with anhydrous ethanol three times;
[0064] (13) The product washed in step (11) and step (12) is placed in a forced air drying oven and dried at 60° C. for 12 h to obtain a microspherical nickel-cobalt-manganese-oxysulfide electrode material.
[0065] Embodiment 2:
[0066] The present embodiment provides a method for preparing a nickel-cobalt-manganese oxysulfide electrode material, including the following specific preparation steps:
[0067] 1) Preparation of nickel-cobalt-manganese oxalate compound precursor
[0068] (1) Dissolve 0.5 mmol nickel nitrate (Ni(NO3)2·6H2O), 2 mmol cobalt nitrate (Co(NO3)2·6H2O), 0.3 mmol manganese acetate (C4H6MnO4·H2O) and 6 mmol oxalic acid (H2C2O4·2H2O) in 80 mL ultrapure water and stir magnetically at room temperature for 8 h;
[0069] (2) washing the product obtained in step (1) with ultrapure water three times;
[0070] (3) washing the product washed in step (2) with anhydrous ethanol three times;
[0071] (4) placing the product washed in step (2) and step (3) in a forced air drying oven and drying at 60° C. for 12 h to obtain a nickel-cobalt-manganese oxalate compound precursor, which is a block-structured ternary metal oxalate compound.
[0072] 2) Preparation of nickel-cobalt-manganese oxysulfide electrode materials
[0073] (1) Weigh 100 mg of the nickel-cobalt-manganese oxalate compound precursor obtained in step 1), evenly disperse it in 60 mL of ultrapure water, add 480 mg of NaOH, and stir at room temperature for 9 h;
[0074] (2) washing the product obtained in step (1) with ultrapure water three times;
[0075] (3) washing the product washed in step (2) with anhydrous ethanol three times;
[0076] (4) placing the product washed in step (2) and step (3) in a forced air drying oven and drying at 60° C. for 12 h to obtain nickel-cobalt-manganese hydroxide, which is a ternary metal hydroxide with a block structure;
[0077] (5) Weigh 20 mg of nickel-cobalt-manganese hydroxide and evenly disperse it in a mixed solution of 3 mL of ultrapure water and 29 mL of N,N-dimethylformamide, and add 40 mg of 2,6-naphthalene dicarboxylic acid;
[0078] (6) The dispersion obtained in step (5) was transferred into a reaction vessel, reacted at 130° C. for 6 h, and then naturally cooled to room temperature;
[0079] (7) washing the product obtained in step (6) with anhydrous ethanol three times;
[0080] (8) placing the product washed in step (7) in a forced air drying oven and drying at 60° C. for 12 h to obtain a nickel-cobalt-manganese-based metal organic framework material with a nanosheet self-assembled microsphere structure;
[0081] (9) Weigh 20 mg of nickel-cobalt-manganese-based metal-organic framework material, evenly disperse it in 60 mL of ultrapure water, and add 100 mg of Na2S·9H2O;
[0082] (10) The dispersion obtained in step (9) was transferred into a reaction vessel, reacted at 90° C. for 6 h, and then naturally cooled to room temperature;
[0083] (11) washing the product obtained in step (10) with ultrapure water three times;
[0084] (12) washing the product washed in step (11) with anhydrous ethanol three times;
[0085] (13) The product washed in step (11) and step (12) is placed in a forced air drying oven and dried at 60° C. for 12 h to obtain a microspherical nickel-cobalt-manganese-oxysulfide electrode material.
[0086] Embodiment 3:
[0087] The present embodiment provides a method for preparing a nickel-cobalt-manganese oxysulfide electrode material, including the following specific preparation steps:
[0088] 1) Preparation of nickel-cobalt-manganese oxalate compound precursor
[0089] (1) Dissolve 2 mmol nickel nitrate (Ni(NO3)2·6H2O), 0.5 mmol cobalt nitrate (Co(NO3)2·6H2O), 0.3 mmol manganese acetate (C4H6MnO4·H2O) and 6 mmol oxalic acid (H2C2O4·2H2O) in 80 mL ultrapure water and stir magnetically at room temperature for 8 h;
[0090] (2) washing the product obtained in step (1) with ultrapure water three times;
[0091] (3) washing the product washed in step (2) with anhydrous ethanol three times;
[0092] (4) placing the product washed in step (2) and step (3) in a forced air drying oven and drying at 60° C. for 12 h to obtain a nickel-cobalt-manganese oxalate compound precursor, which is a block-structured ternary metal oxalate compound.
[0093] 2) Preparation of nickel-cobalt-manganese oxysulfide electrode materials
[0094] (1) Weigh 100 mg of the nickel-cobalt-manganese oxalate compound precursor obtained in step 1), evenly disperse it in 60 mL of ultrapure water, add 400 mg of NaOH, and stir at room temperature for 13 h;
[0095] (2) washing the product obtained in step (1) with ultrapure water three times;
[0096] (3) washing the product washed in step (2) with anhydrous ethanol three times;
[0097] (4) placing the product washed in step (2) and step (3) in a forced air drying oven and drying at 60° C. for 12 h to obtain nickel-cobalt-manganese hydroxide, which is a ternary metal hydroxide with a block structure;
[0098] (5) Weigh 20 mg of nickel-cobalt-manganese hydroxide and evenly disperse it in a mixed solution of 3 mL of ultrapure water and 29 mL of N,N-dimethylformamide, and add 80 mg of 2,6-naphthalene dicarboxylic acid;
[0099] (6) The dispersion obtained in step (5) was transferred into a reaction vessel, reacted at 130° C. for 6 h, and then naturally cooled to room temperature;
[0100] (7) washing the product obtained in step (6) with anhydrous ethanol three times;
[0101] (8) placing the product washed in step (7) in a forced air drying oven and drying at 60° C. for 12 h to obtain a nickel-cobalt-manganese-based metal organic framework material with a nanosheet self-assembled microsphere structure;
[0102] (9) Weigh 20 mg of NiCoMn-based metal organic framework material, evenly disperse it in 60 mL of ultrapure water, and add 120 mg of Na2S·9H2O;
[0103] (10) The dispersion obtained in step (9) was transferred into a reaction vessel, reacted at 90° C. for 6 h, and then naturally cooled to room temperature;
[0104] (11) washing the product obtained in step (10) with ultrapure water three times;
[0105] (12) washing the product washed in step (11) with anhydrous ethanol three times;
[0106] (13) placing the product washed in step (11) and step (12) in a forced air drying oven and drying at 60° C. for 12 h to obtain a microspherical nickel-cobalt-manganese-oxysulfide electrode material;
[0107] Embodiment 4:
[0108] The present embodiment provides a method for preparing a nickel-cobalt-manganese oxysulfide electrode material, including the following specific preparation steps:
[0109] 1) Preparation of nickel-cobalt-manganese oxalate compound precursor:
[0110] (1) Dissolve 2 mmol nickel nitrate (Ni(NO3)2·6H2O), 0.5 mmol cobalt nitrate (Co(NO3)2·6H2O), 0.3 mmol manganese acetate (C4H6MnO4·H2O) and 6 mmol oxalic acid (H2C2O4·2H2O) in 80 mL ultrapure water and stir magnetically at room temperature for 8 h;
[0111] (2) washing the product obtained in step (1) with ultrapure water three times;
[0112] (3) washing the product washed in step (2) with anhydrous ethanol three times;
[0113] (4) placing the product washed in step (2) and step (3) in a forced air drying oven and drying at 60° C. for 12 h to obtain a nickel-cobalt-manganese oxalate compound precursor, which is a block-structured ternary metal oxalate compound.
[0114] 2) Preparation of nickel-cobalt-manganese oxysulfide electrode materials:
[0115] (1) Weigh 100 mg of the nickel-cobalt-manganese oxalate compound precursor obtained in step 1), evenly disperse it in 60 mL of ultrapure water, add 320 mg of NaOH, and stir at room temperature for 13 h;
[0116] (2) washing the product obtained in step (1) with ultrapure water three times;
[0117] (3) washing the product washed in step (2) with anhydrous ethanol three times;
[0118] (4) placing the product washed in step (2) and step (3) in a forced air drying oven and drying at 60° C. for 12 h to obtain nickel-cobalt-manganese hydroxide, which is a ternary metal hydroxide with a block structure;
[0119] (5) Weigh 20 mg of nickel-cobalt-manganese hydroxide and evenly disperse it in a mixed solution of 3 mL of ultrapure water and 29 mL of N,N-dimethylformamide, and add 120 mg of 2,6-naphthalene dicarboxylic acid;
[0120] (6) The dispersion obtained in step (5) was transferred into a reaction vessel, reacted at 130° C. for 6 h, and then naturally cooled to room temperature;
[0121] (7) washing the product obtained in step (6) with anhydrous ethanol three times;
[0122] (8) placing the product washed in step (7) in a forced air drying oven and drying at 60° C. for 12 h to obtain a nickel-cobalt-manganese-based metal organic framework material with a nanosheet self-assembled microsphere structure;
[0123] (9) Weigh 20 mg of NiCoMn-based metal organic framework material, evenly disperse it in 60 mL of ultrapure water, and add 120 mg of Na2S·9H2O;
[0124] (10) The dispersion obtained in step (9) was transferred into a reaction vessel, reacted at 90° C. for 6 h, and then naturally cooled to room temperature;
[0125] (11) washing the product obtained in step (10) with ultrapure water three times;
[0126] (12) washing the product washed in step (11) with anhydrous ethanol three times;
[0127] (13) The product washed in step (11) and step (12) is placed in a forced air drying oven and dried at 60° C. for 12 h to obtain a microspherical nickel-cobalt-manganese-oxysulfide electrode material.
[0128] Embodiment 5:
[0129] The present embodiment provides a method for preparing a nickel-cobalt-manganese oxysulfide electrode material, including the following specific preparation steps:
[0130] 1) Preparation of nickel-cobalt-manganese oxalate compound precursor:
[0131] (1) Dissolve 2 mmol nickel nitrate (Ni(NO3)2·6H2O), 1 mmol cobalt nitrate (Co(NO3)2·6H2O), 0.5 mmol manganese acetate (C4H6MnO4·H2O) and 6 mmol oxalic acid (H2C2O4·2H2O) in 80 mL ultrapure water and stir magnetically at room temperature for 8 h;
[0132] (2) washing the product obtained in step (1) with ultrapure water three times;
[0133] (3) washing the product washed in step (2) with anhydrous ethanol three times;
[0134] (4) placing the product washed in step (2) and step (3) in a forced air drying oven and drying at 60° C. for 12 h to obtain a nickel-cobalt-manganese oxalate compound precursor, which is a block-structured ternary metal oxalate compound.
[0135] 2) Preparation of nickel-cobalt-manganese oxysulfide electrode materials:
[0136] (1) Weigh 100 mg of the nickel-cobalt-manganese oxalate compound precursor obtained in step 1), evenly disperse it in 60 mL of ultrapure water, add 240 mg of NaOH, and stir at room temperature for 17 h;
[0137] (2) washing the product obtained in step (1) with ultrapure water three times;
[0138] (3) washing the product washed in step (2) with anhydrous ethanol three times;
[0139] (4) placing the product washed in step (2) and step (3) in a forced air drying oven and drying at 60° C. for 12 h to obtain nickel-cobalt-manganese hydroxide, which is a ternary metal hydroxide with a block structure;
[0140] (5) Weigh 20 mg of nickel-cobalt-manganese hydroxide and evenly disperse it in a mixed solution of 3 mL of ultrapure water and 29 mL of N,N-dimethylformamide, and add 160 mg of 2,6-naphthalene dicarboxylic acid;
[0141] (6) The dispersion obtained in step (5) was transferred into a reaction vessel, reacted at 130° C. for 6 h, and then naturally cooled to room temperature;
[0142] (7) washing the product obtained in step (6) with anhydrous ethanol three times;
[0143] (8) placing the product washed in step (7) in a forced air drying oven and drying at 60° C. for 12 h to obtain a nickel-cobalt-manganese-based metal organic framework material with a nanosheet self-assembled microsphere structure;
[0144] (9) Weigh 20 mg of NiCoMn-based metal organic framework material, evenly disperse it in 60 mL of ultrapure water, and add 140 mg of Na2S·9H2O;
[0145] (10) The dispersion obtained in step (9) was transferred into a reaction vessel, reacted at 90° C. for 6 h, and then naturally cooled to room temperature;
[0146] (11) washing the product obtained in step (10) with ultrapure water three times;
[0147] (12) washing the product washed in step (11) with anhydrous ethanol three times;
[0148] (13) The product washed in step (11) and step (12) is placed in a forced air drying oven and dried at 60° C. for 12 h to obtain a microspherical nickel-cobalt-manganese-oxysulfide electrode material.
[0149] See attached Figure 1 , Attachment Figure 2 , Attachment Figure 3 and attached Figure 4As shown, the nickel cobalt manganese oxalate compound, nickel cobalt manganese hydroxide, nickel cobalt manganese-based metal organic framework and nickel cobalt manganese oxysulfide prepared in Example 4 of the present invention were characterized by scanning electron microscopy (SEM); the nickel cobalt manganese oxalate compound precursor was a stable block structure; the nickel cobalt manganese hydroxide maintained structural characteristics similar to the precursor; after reacting with 2,6-naphthalene dicarboxylic acid under hydrothermal conditions, the nickel cobalt manganese-based metal organic framework exhibited a spherical structure of nanosheet self-assembly, indicating that the preparation step can significantly improve the morphology of the material; after sulfurization treatment, the synthesized nickel cobalt manganese oxysulfide electrode material retained the spherical structure, but its surface was relatively rough, and a small part of the sheet structure of the metal organic framework material was still maintained, which is more conducive to the full contact between the electrolyte solution and the material, and promotes the electrochemical energy storage process.
[0150] See attached Figure 5 , Attachment Figure 6 and attached Figure 7 As shown, the nickel cobalt manganese oxalate compound, nickel cobalt manganese hydroxide, nickel cobalt manganese-based metal organic framework and nickel cobalt manganese oxysulfide prepared in Example 4 of the present invention were characterized by X-ray diffraction (XRD). Analysis showed that the characteristic peaks of the nickel cobalt manganese oxalate compound were consistent with NiC2O4·2H2O (JCPDS14-0742), CoC2O4·2H2O (JCPDS25-0250) and MnC2O4·2H2O (JCPDS25-0544), and the diffraction peaks on the XRD spectrum of nickel cobalt manganese hydroxide corresponded to the crystal planes (003), (006), (012), (015), (018), (110) and (202) crystal planes. For the XRD spectrum of nickel cobalt manganese oxysulfide, the characteristic peak of the sulfide is not obvious. The two relatively obvious characteristic peaks in the spectrum can correspond to the (012) and (110) crystal planes of the hydroxide, indicating that the material is a composite material of oxide and sulfide. The composition and crystal form of the nickel cobalt manganese oxalate compound precursor, intermediate product and nickel cobalt manganese oxysulfide can be determined by XRD characterization analysis.
[0151] See attached Figure 8 As shown, the nickel-cobalt-manganese oxysulfide electrode material prepared in Example 4 of the present invention is subjected to X-ray photoelectron spectroscopy (XPS). It can be seen from the figure that the material is mainly composed of nickel, cobalt, manganese, oxygen, sulfur and carbon elements, wherein oxygen exists in the form of -2-valent oxygen, COC and -C=O in the compound, sulfur is mainly -2-valent sulfur in the compound, and carbon exists in the form of OC=O, CO, and C=C; the above characterization results indicate that the material is a composite material of nickel-cobalt-manganese oxide and sulfide, and that a certain amount of carbon doping exists in the material.
[0152] See attached Fig. 9As shown, the nickel-cobalt-manganese-oxysulfide electrode material prepared in Example 4 of the present invention was subjected to a cyclic voltammetry test. The test adopted a three-electrode system, with the prepared material as the working electrode, the platinum electrode as the counter electrode, the Hg / HgO electrode as the reference electrode, and 2 molL -1 KOH solution is the electrolyte solution. The test results show that at different scan rates, the cyclic voltammetry curves obtained all have obvious redox peaks, which preliminarily determines that the composite material is a battery-type energy storage material; in addition, as the scan rate increases, the cyclic voltammetry curves still maintain similar shape characteristics, only the redox peak position has a certain shift, and the integral area of the curve has increased significantly, which indicates that the material has excellent reversibility during the energy storage process.
[0153] See attached Fig.10 As shown, the nickel-cobalt-manganese oxysulfide electrode material prepared in Example 4 of the present invention was subjected to constant current charge-discharge test, and the test system was the same as the cyclic voltammetry test. As can be seen from the figure, at different current densities, the constant current charge-discharge curves obtained have obvious charge-discharge platforms, further indicating that the prepared material is a battery-type energy storage material, which is consistent with the cyclic voltammetry test analysis. Calculations show that at 1Ag -1 , 2Ag -1 , 3Ag -1 , 5Ag -1 , 8Ag -1 , 10Ag -1 , 15Ag -1 , and 20Ag -1 At the current density, the specific capacitance of the material is 1488Fg -1 、1388Fg -1 ,1276Fg -1 ,1148Fg -1 、995Fg -1 、921Fg -1 、735Fg -1 and 612Fg -1 , the results show that the prepared nickel-cobalt-manganese oxysulfide has excellent charge storage capacity.
[0154] In summary, the present invention uses a simple chemical precipitation method to achieve the large-scale preparation of a nickel-cobalt-manganese ternary oxalic acid compound precursor with controllable composition and structure at room temperature, and then further prepares it into a nickel-cobalt-manganese-based metal-organic framework material, effectively regulating the composition and morphology of the material, and finally uses an anion exchange method to prepare the corresponding carbon-doped nickel-cobalt-manganese oxysulfide composite electrode material. The present invention determines the material preparation method by rationally designing the preparation process, adjusting the reaction parameters, and obtains a high-performance supercapacitor electrode material based on the material composition and structure regulation. The material prepared by the present invention has good application prospects, and the proposed composite electrode material preparation method is scientific and reasonable, has strong applicability, and has good effects, and is particularly suitable for preparing high-performance electrode materials.
[0155] The above is only a preferred embodiment of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A nickel-cobalt-manganese oxysulfide electrode material, characterized in that In the nickel-cobalt-manganese oxysulfide electrode material, the atomic ratio of nickel, cobalt and manganese is 2:0.5:0.3, and the nickel-cobalt-manganese oxysulfide electrode material is a micron-scale spherical structure, and the diameter of the micron-scale spherical structure is 2 to 9 um; The nickel-cobalt-manganese-oxysulfide electrode material is prepared by the following steps: 1) Preparation of nickel-cobalt-manganese oxalate compound precursor: 1.1) Dissolve Ni(NO3)2·6H2O and Co(NO3)2·6H2O in a molar ratio of 1:4 to 4:1, Ni(NO3)2·6H2O and C4H6MnO4·H2O in a molar ratio of 1:0.05 to 1:0.25, and Ni(NO3)2·6H2O and H2C2O4·2H2O in a molar ratio of 1:12 to 1:3 in 80 mL of ultrapure water and stir magnetically for 8 h at room temperature; 1.2) Wash the product obtained in step 1.1) with ultrapure water three times; 1.3) Wash the product obtained in step 1.2) with anhydrous ethanol three times; 1.4) The product obtained in step 1.3) was placed in a forced air drying oven and dried at 60°C for 12 h to obtain a nickel-cobalt-manganese oxalate compound precursor; 2) Preparation of nickel-cobalt-manganese oxysulfide electrode materials: 2.1) Weigh 100 mg of the nickel-cobalt-manganese oxalate compound precursor obtained in step 1.4) and evenly disperse it in 60 mL of ultrapure water. Add 240 to 640 mg of NaOH and stir at room temperature for 5 to 17 h. 2.2) Wash the product obtained in step 2.1) with ultrapure water three times; 2.3) Wash the product obtained in step 2.2) with anhydrous ethanol three times; 2.4) The product obtained in step 2.3) was placed in a forced air drying oven at 60°C for 12 h to obtain nickel-cobalt-manganese hydroxide; 2.5) Weigh 20 mg of the nickel-cobalt-manganese hydroxide obtained in step 2.4) and evenly disperse it in a mixed solution of 3 mL of ultrapure water and 29 mL of N,N-dimethylformamide, and add 20-160 mg of 2,6-naphthalene dicarboxylic acid to obtain a dispersion; 2.6) The dispersion obtained in step 2.5) was transferred into a reaction vessel, reacted at 130 °C for 6 h, and then naturally cooled to 25 °C; 2.7) Wash the product obtained in step 2.6) with anhydrous ethanol three times; 2.8) The product obtained in step 2.7) was placed in a forced air drying oven and dried at 60°C for 12 h to obtain a nanosheet self-assembled microsphere structured nickel-cobalt-manganese-based metal organic framework material; 2.9) Weigh the nanosheet self-assembled microsphere structure nickel-cobalt-manganese-based metal organic framework material obtained in step 2.8), evenly disperse it in 60 mL ultrapure water, and add 80-140 mg Na2S·9H2O; 3.0) The dispersion obtained in step 2.9) was transferred into a reaction vessel, reacted at 90 °C for 6 h, and then naturally cooled to 25 °C; 3.1) Wash the product obtained in step 3.0) three times with ultrapure water; 3.2) Wash the product obtained in step 3.1) with anhydrous ethanol three times; 3.3) The product obtained in step 3.2) was placed in a forced air drying oven and dried at 60°C for 12 h to obtain a nickel-cobalt-manganese oxysulfide electrode material.
2. The nickel-cobalt-manganese oxysulfide electrode material according to claim 1, characterized in that: In the nickel-cobalt-manganese oxysulfide electrode material, the atomic ratio of nickel to sulfur is 1:1, 1:1.14 or 1:
2.
3. A method for preparing a nickel-cobalt-manganese oxysulfide electrode material, characterized in that: It includes the following steps: 1) Preparation of nickel-cobalt-manganese oxalate compound precursor: 1.1) Dissolve Ni(NO3)2·6H2O and Co(NO3)2·6H2O in a molar ratio of 1:4 to 4:1, Ni(NO3)2·6H2O and C4H6MnO4·H2O in a molar ratio of 1:0.05 to 1:0.25, and Ni(NO3)2·6H2O and H2C2O4·2H2O in a molar ratio of 1:12 to 1:3 in 80 mL of ultrapure water and stir magnetically for 8 h at room temperature; 1.2) Wash the product obtained in step 1.1) with ultrapure water three times; 1.3) Wash the product obtained in step 1.2) with anhydrous ethanol three times; 1.4) The product obtained in step 1.3) was placed in a forced air drying oven and dried at 60°C for 12 h to obtain a nickel-cobalt-manganese oxalate compound precursor; 2) Preparation of nickel-cobalt-manganese oxysulfide electrode materials: 2.1) Weigh 100 mg of the nickel-cobalt-manganese oxalate compound precursor obtained in step 1.4) and evenly disperse it in 60 mL of ultrapure water. Add 240 to 640 mg of NaOH and stir at room temperature for 5 to 17 h. 2.2) Wash the product obtained in step 2.1) with ultrapure water three times; 2.3) Wash the product obtained in step 2.2) with anhydrous ethanol three times; 2.4) The product obtained in step 2.3) was placed in a forced air drying oven at 60°C for 12 h to obtain nickel-cobalt-manganese hydroxide; 2.5) Weigh 20 mg of the nickel-cobalt-manganese hydroxide obtained in step 2.4) and evenly disperse it in a mixed solution of 3 mL of ultrapure water and 29 mL of N,N-dimethylformamide, and add 20-160 mg of 2,6-naphthalene dicarboxylic acid to obtain a dispersion; 2.6) The dispersion obtained in step 2.5) was transferred into a reaction vessel, reacted at 130 °C for 6 h, and then naturally cooled to 25 °C; 2.7) Wash the product obtained in step 2.6) with anhydrous ethanol three times; 2.8) The product obtained in step 2.7) was placed in a forced air drying oven and dried at 60°C for 12 h to obtain a nanosheet self-assembled microsphere structured nickel-cobalt-manganese-based metal organic framework material; 2.9) Weigh the nanosheet self-assembled microsphere structure nickel-cobalt-manganese-based metal organic framework material obtained in step 2.8), evenly disperse it in 60 mL ultrapure water, and add 80-140 mg Na2S·9H2O; 3.0) The dispersion obtained in step 2.9) was transferred into a reaction vessel, reacted at 90 °C for 6 h, and then naturally cooled to 25 °C; 3.1) Wash the product obtained in step 3.0) three times with ultrapure water; 3.2) Wash the product obtained in step 3.1) with anhydrous ethanol three times; 3.3) The product obtained in step 3.2) was placed in a forced air drying oven and dried at 60°C for 12 h to obtain a nickel-cobalt-manganese oxysulfide electrode material.
4. The method for preparing a nickel-cobalt-manganese oxysulfide electrode material according to claim 3, characterized in that In the step 1.4), the nickel-cobalt-manganese oxalate compound precursor is a ternary metal oxalate compound with a block structure.
5. The method for preparing a nickel-cobalt-manganese oxysulfide electrode material according to claim 3, characterized in that: In the step 2.4), the nickel-cobalt-manganese hydroxide is a ternary metal hydroxide with a block structure.
6. The method for preparing a nickel-cobalt-manganese oxysulfide electrode material according to claim 3, characterized in that: In the steps 2.6) and 3.0), the reactor is a stainless steel reactor lined with polytetrafluoroethylene.