A preparation method of a novel block-shaped xenogeneic bone repair material

By using an azeotropic mixture of ethylenediamine with ethylene glycol monomethyl ether, n-butanol, or isobutanol, and low-temperature calcination technology, the problems of immune rejection and structural changes in xenogeneic bone materials were solved, and a highly efficient and safe block bone repair material was prepared.

CN116036377BActive Publication Date: 2024-11-05SHAANXI RUISHENG BIOTECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310277158.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-21
Publication Date
2024-11-05
Estimated Expiration
2043-03-21

AI Technical Summary

Technical Problem

Existing xenogeneic bone materials suffer from immune rejection issues during preparation. High-temperature calcination alters the bone mineral structure, and granular materials cannot effectively maintain osteogenic space. Furthermore, the preparation process is inefficient.

Method used

Ethylenediamine is used to form an azeotropic mixture with ethylene glycol monomethyl ether, n-butanol or isobutanol to remove fat and protein simultaneously. Combined with low-temperature calcination technology at 250-350℃, the porous structure of bone is preserved and the mechanical strength is improved.

Benefits of technology

It achieves efficient removal of organic matter, preserves the natural bone structure, improves preparation efficiency, has good biocompatibility and space support effect, and avoids structural changes caused by high-temperature calcination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116036377B_ABST
    Figure CN116036377B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a novel block-shaped xenogeneic bone repair material; the material is prepared by the following steps in sequence: material selection, disinfection, defatting and deproteinization, calcination, drying, and sterilization. The method involved in the present invention is to use an azeotropic mixture of an alkaline reagent ethylenediamine and ethylene glycol monomethyl ether, n-butanol, and isobutanol to remove organic matter at the same time. In addition, the boiling point is increased, which not only significantly shortens the process time and reduces the production cost, thereby improving the production efficiency; at the same time, the natural structure of the bone is retained, ensuring that the crystallinity of the apatite crystals in the bone body is not significantly affected; in addition, compared with granular bone transplant materials, block bones can play a good spatial support effect. The product prepared by the method of the present invention not only has a natural multi-porous three-dimensional spatial structure similar to human bones and a highly similar phase composition; but also has the advantages of high specific surface area, low immunogenicity, high safety, and good biocompatibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of material preparation methods, and in particular relates to a method for preparing a novel block-shaped heterogeneous bone repair material. Background Art

[0002] For the human body, many factors can lead to problems such as jaw bone deficiency and insufficiency. For example, trauma, infection, tumor resection, congenital diseases, etc., will not only have adverse effects on the human facial morphology and function, but also increase the difficulty of implanting and repairing defective teeth. For patients who need oral implant restoration, sufficient bone volume is a prerequisite for obtaining good functional and aesthetic effects. Therefore, when there is a severe horizontal bone defect in the alveolar ridge or a vertical bone defect at the same time, bone augmentation repair is required.

[0003] Autologous bone is considered the "gold standard" of bone graft materials because of its good osteogenicity, osteoconductivity and osteoinductivity. However, autologous bone transplantation often requires the opening of a second surgical site in clinical practice. If an intraoral donor site is selected, the available bone volume is very limited; if an extraoral donor site is selected, there is also a risk of additional complications. Allogeneic bone is closest to autologous bone in performance. In recent years, block allogeneic grafts are often used to repair alveolar ridge height defects or severe alveolar ridge atrophy in order to provide sufficient bone volume for implants. However, there are also problems in ethics and immunogenicity. In addition, allogeneic bone blocks are limited by different materials: such as young and old, male and female, and the problem of material supply, resulting in limited production capacity, different absorption, and ultimately unstable clinical effects.

[0004] Therefore, in order to solve the problem of bone transplantation, it is very necessary to develop research on bone substitute materials. Among them, animal-derived xenogeneic bones are widely used in research because of their wide and unrestricted sources, low manufacturing costs, and easy access and processing. However, animal-derived bone materials are xenogeneic materials for the human body and have a strong immune rejection problem. The antigens of xenogeneic bones are mainly located in the organic matter of the bones. Therefore, removing organic matter is an indispensable process for eliminating the antigenicity of xenogeneic transplanted bones. In the process of removing antigens from xenogeneic bones, organic components such as fat and protein need to be removed. The commonly used methods are high-temperature calcination and organic reagent methods, but both have the following shortcomings.

[0005] Although high-temperature calcination can completely remove organic matter, it will cause significant changes in the bone mineral structure, such as increased crystallinity and reduced porosity, which will lead to significant changes in the performance of bone materials. In addition, carbonate ions in xenogeneic bone materials have the function of regulating material degradation, and high-temperature calcination will cause the decomposition of carbonate ions, further resulting in the material being unable to degrade in the body.

[0006] Organic reagent method, currently the commonly used method is a step-by-step method to remove fat and protein separately, that is, first de-fat, then de-protein. The most representative process is the Bio-Oss product, which uses a step-by-step method to remove organic components (fat and protein), specifically: using the organic solvent toluene to remove fat, and after degreasing, using ethylenediamine to remove protein. Deproteinization is the use of ethylenediamine and water to form an azeotropic mixture. Since the deproteinization effect of ethylenediamine is positively correlated with the action temperature, the higher the temperature, the stronger the effect. The boiling point of the mixture of ethylenediamine and water is low, resulting in the need for bone meal to boil in the ethylenediamine aqueous solution for 50 hours. This method has the disadvantages of long construction period, high cost, and low efficiency.

[0007] At present, most commonly used xenogeneic bone products are in granular form. When there are severe and obvious horizontal and vertical bone defects in the alveolar bone, the remaining alveolar ridge cannot provide sufficient retention for the granular bone graft material during bone augmentation repair, which can easily cause displacement and spatial collapse of the granular bone graft material and fail to maintain a good bone formation space. Block bone transplantation can provide good spatial support, and its stability is conducive to the completion of vascularization and "creeping replacement", which has irreplaceable advantages.

[0008] In view of the above problems, it is necessary to further improve the process and prepare a satisfactory block-shaped xenogeneic bone repair material that is non-immunogenic and retains the natural bone structure. Summary of the invention

[0009] The purpose of the present invention is to provide a method for preparing a novel block-shaped heterogeneous bone repair material.

[0010] The present invention provides an efficient preparation method for heterogeneous block bone transplant materials. The following ratios are used: 10%-20% ethylene glycol monomethyl ether, 10%-30% n-butanol and 50%-80% ethylenediamine azeotropic mixture, or 10%-30% ethylene glycol monomethyl ether, 20%-30% isobutyl alcohol and 40%-70% ethylenediamine azeotropic mixture. The organic components (fat and protein) are removed simultaneously by using the principle that organic solvents and fats are similarly soluble in each other to remove fats, and the amino groups of ethylenediamine react with the amide bonds of proteins to remove proteins. In addition, its boiling point is significantly higher than that of the mixture of ethylenediamine and water, which enhances the deproteinization effect, and ethylene glycol monomethyl ether also has the function of increasing the boiling point. The process significantly shortens the process time, reduces the production of finished products, and improves efficiency.

[0011] The method of the present invention further calcines at 250-350°C and solidifies the material to improve the compressive strength of the bone repair material, and also makes the microporous (<10um) structure appear, while avoiding the disadvantages of high-temperature calcination (crystallinity, porosity). The material retains the natural multi-porous three-dimensional spatial structure similar to human bone and the highly similar phase composition, and has the advantages of high specific surface area, low immunogenicity, high safety, good biocompatibility, etc., and perfectly overcomes the problems of spatial collapse and inability to maintain bone formation space in granular bone transplant materials.

[0012] The present invention is achieved through the following technical solutions:

[0013] The present invention relates to a method for preparing a novel block-shaped xenogeneic bone repair material, comprising the following steps:

[0014] Step 1, using a bone saw to cut the distal cancellous bone of the bovine femoral epiphysis, removing the accessory tissues around the lamellar cancellous bone with the bone saw, and then cutting into bone blocks of (5-10)×(5-10)×(5-30) mm.

[0015] Step 2, the specific steps of disinfection are: put the selected block bone into a clean container, add 2-5 times the amount (the mass volume ratio of the block bone to ethanol is 1: (2-5), such as: the bone block is 100g, and the ethanol is 200-500ml.) of 75% ethanol, soak for 30 minutes, and drain; (2) put the bone block into a clean container again, weigh 15 times the amount (the mass volume ratio of the block bone to purified water is 1:15) of purified water, and add it to the container; (3) ultrasonic cleaning 3 times, each time for 10 minutes; this step is to immerse in an ethanol solution. When the bone block is immersed in an ethanol solution, ethanol has strong volatility and can absorb the moisture of bacterial protein, causing it to dehydrate and solidify, thereby achieving the purpose of killing bacteria; at the same time, ethanol can dissolve the fat tissue on the surface of the bone tissue, playing a role of partial degreasing.

[0016] Step 3, defatting and deproteinizing: The specific steps of defatting and deproteinizing are as follows: put the unsterilized block bone into the flask of the extraction equipment and then add the azeotropic mixture of ethylenediamine and ethylene glycol monomethyl ether, n-butanol and isobutanol; Soxhlet extraction for 5-7 hours; after defatting and deproteinizing, put the bone block into a clean container and weigh it, then add 20 times the amount (the mass volume ratio of the block bone to 75% ethanol is 1:20) of 75% ethanol, and ultrasonically clean it 3 times, each time for 10 minutes. Then wash it under running water for 2 hours until it is neutral; dry the bone block at 90°C in an oven for 4 hours. The defatting and deproteinizing involved in this step is an important process to remove the organic phase from the bone. The retention of organic components increases the risk of immunogenicity. Although the high-temperature calcination method can completely remove organic matter, it will cause significant changes in the crystal structure of bone minerals, such as crystallinity, porosity, etc., which will lead to significant changes in the properties of bone materials. In addition, carbonate ions in xenogeneic bone materials have the function of regulating material degradation, and high-temperature calcination will lead to the decomposition of carbonate ions, further causing the material to be unable to degrade in the body.

[0017] Step 4, calcination: bones are composed of organic and inorganic substances. Organic substances determine their toughness, while inorganic substances determine their hardness. When the organic components are removed, the inorganic salt components are loosely bonded and the mechanical strength is reduced. It is necessary to enhance the mechanical strength and solidify it only by low-temperature calcination to increase the mechanical strength of the bone material. In the subsequent cooling process, it should be avoided to suddenly remove the bone blocks from the muffle furnace and cool them to avoid the formation of a "cold bridge", which will cause the calcined bone structure to lose its firmness. It would be more beneficial to slowly cool the bone material by closing the furnace to reduce the temperature in the muffle furnace. Among them, the slow cooling step includes cooling for about 24 hours to prevent stress, cracks or brittleness; the calcination temperature is 250-350°C, and the calcination time is 10-20h.

[0018] The calcination step involved in the present invention is an indispensable process. The calcination temperature of the present invention is 250-350°C to achieve the purpose of the present invention. If the calcination temperature is lower than 250°C, the curing effect is poor, the mechanics is reduced, and the compression resistance of the bone material is poor. In addition, the residual trace protein cannot be decomposed, so that the micropores (<10um) cannot be revealed. The function of the microporous structure is to facilitate the adhesion and enrichment of growth factors, the penetration of body fluids, and the absorption and degradation. The inability to show the microporous structure will affect the capillary siphon performance and hydrophilicity of the material and affect the degradation rate. In addition, the microporous structure also determines the specific surface area of ​​the material. A larger specific surface area increases the contact area between the material and cells and body fluids, which is conducive to the adhesion and growth of bone cells. A reduction in the amount of micropores will lead to a reduction in the specific surface area.

[0019] If the calcination temperature is higher than 350°C, crystal growth will occur, which will reduce the porosity of natural bone and increase the crystallinity. The increase in crystallinity will directly affect the degradation rate. The higher the crystallinity, the more difficult it is to degrade, resulting in a mismatch between the degradation rate and the growth rate of new bone. Low porosity will affect cell growth and migration, nutrient delivery, and vascularization.

[0020] In summary, the calcination temperature of the method of the present invention is 250-350° C. If the temperature is higher or lower than this range, the final technical effect of the present invention cannot be achieved.

[0021] Step 5, drying: After the bone material is cleaned, it must be dried for easy storage. The cleaned bone material is placed in a 90°C oven to dry for 4-5 hours.

[0022] Step 6, packaging, encapsulating and sterilizing the dried bone blocks.

[0023] The present invention has the following advantages:

[0024] (1) The present invention provides an efficient preparation method for heterogeneous block bone transplant materials, which utilizes the azeotropic mixture formed by ethylenediamine and ethylene glycol monomethyl ether, n-butanol or isobutanol, utilizes the principle that organic solvents and fats are similarly miscible to remove fats, and the amino groups of ethylenediamine react with the amide bonds of proteins to remove proteins, and simultaneously removes organic components (fat and protein); in addition, its boiling point is significantly higher than that of the mixture of ethylenediamine and water, which enhances the deproteinization effect, wherein ethylene glycol monomethyl ether also has the function of increasing the boiling point. This process not only significantly shortens the process time, reduces the production of finished products, and improves efficiency, but also can more effectively remove organic matter and immunogens, and solve the risk of immunogenicity; it also retains the natural structure of the bone, ensuring that the crystallinity of the apatite crystals in the bone body is not significantly affected; it also avoids changes in structure and function caused by high-temperature calcination. In addition, compared with granular bone transplant materials, block bone transplants can have a good spatial support effect.

[0025] (2) The method involved in the present invention is a highly efficient degreasing and deproteinizing method; the product prepared by this method not only has a natural porous three-dimensional spatial structure similar to human bones and a highly similar phase composition; but also has the advantages of high specific surface area, low immunogenicity, high safety, good biocompatibility, etc.

[0026] (3) The method involved in the present invention is a method for preparing a heterogeneous block bone transplant material, which overcomes the problems of space collapse and inability to maintain bone formation space in granular bone transplant materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a rendering of a bone block prepared by the method of the present invention;

[0028] Figure 2 This is a scanning electron microscope (50 times) image of a bone block prepared by the method of the present invention;

[0029] Figure 3 The bone block pore structure is prepared by the method of the present invention;

[0030] Figure 4 is the XRD spectrum of the bone block prepared by the method involved in the present invention;

[0031] Figure 5 The cell morphology of the cytotoxicity test involved in the present invention;

[0032] Figure 6 It is the cell proliferation rate in the cytotoxicity test involved in the present invention. DETAILED DESCRIPTION

[0033] The present invention is described in detail below in conjunction with specific embodiments. It should be noted that the following embodiments are only further descriptions of the present invention, but the protection scope of the present invention is not limited to the following embodiments.

[0034] Example 1

[0035] This embodiment relates to a method for preparing a novel block-shaped xenogeneic bone repair material, comprising the following steps:

[0036] 1. Materials taken:

[0037] Wearing work clothes, use a bone saw to cut the cancellous bone at the distal end of the bovine femoral epiphysis, use the bone saw to remove the accessory tissue around the flaky cancellous bone, and then cut it into bone blocks of (5-10)×(5-10)×(5-30) mm.

[0038] 2. Disinfection:

[0039] Place the cancellous bone block in a clean container, add 2 times the volume (mass volume ratio of the block bone to ethanol is 1:2) of 75% ethanol, soak for 30 minutes, and drain; place the bone block in a clean container, weigh 15 times the volume (mass volume ratio of the block bone to purified water is 1:15) of purified water, and add it to the container. Perform ultrasonic cleaning 3 times, 10 minutes each time.

[0040] 3. Remove organic matter

[0041] Take the above disinfected bone block, put it in a flask, and then add the azeotropic mixture of 70% ethylenediamine, 10% ethylene glycol monomethyl ether, and 20% n-butanol; Soxhlet extraction for 5 hours, changing the liquid once an hour; after completion, put the bone block in a clean container and weigh it, then add 20 times the amount (the mass volume ratio of the block bone to 75% ethanol is 1:20) of 75% ethanol, and ultrasonically clean it 3 times, 10 minutes each time. Then wash it under running water for 2 hours until it is neutral. Dry the bone block in an oven, drying conditions: 90°C, drying for 4 hours. Among them, the mass volume ratio of the bone block to the azeotropic mixture is 1:10.

[0042] 4. Calcination

[0043] Place the bone blocks flat on a stainless steel tray and then place them in a muffle furnace. Set the calcination parameters to 250°C for 20 hours. The heating process is not included in the calcination time, and the cooling process is to close the furnace door and cool naturally.

[0044] 5. Drying

[0045] The calcined bone blocks were washed with ultrapure water and then placed in a forced air drying oven at 90°C for 4 hours.

[0046] 6. Sterilization

[0047] The dried bone blocks are packaged, encapsulated, and sterilized (cobalt-60 radiation sterilization, with an irradiation dose of 25 KGy).

[0048] Example 2

[0049] This embodiment relates to a method for preparing a novel block-shaped xenogeneic bone repair material, comprising the following steps:

[0050] 1. Materials taken:

[0051] Wearing work clothes, use a bone saw to cut the cancellous bone at the distal end of the bovine femoral epiphysis, use the bone saw to remove the accessory tissue around the flaky cancellous bone, and then cut it into bone blocks of (5-10)×(5-10)×(5-30) mm.

[0052] 2. Disinfection:

[0053] Place the cancellous bone block in a clean container, add 5 times the volume (mass volume ratio of the block bone to ethanol is 1:5) of 75% ethanol, soak for 30 minutes, drain, place the bone block in a clean container, weigh 15 times the volume (mass volume ratio of the block bone to purified water is 1:15) of purified water, add to the container. Perform ultrasonic cleaning 3 times, 10 minutes each time.

[0054] 3. Remove organic matter

[0055] Take the above disinfected bone blocks, put them into a flask, and then add 50% ethylenediamine, 20% ethylene glycol monomethyl ether, and 30% n-butanol to form an azeotropic mixture; Soxhlet extraction for 6 hours, changing the liquid once an hour; after completion, put the bone blocks into a clean container and weigh them, then add 20 times the amount (the mass volume ratio of block bone to 75% ethanol is 1:20) of 75% ethanol, and ultrasonically clean them 3 times, 10 minutes each time. Then wash them under running water for 2 hours until they are neutral. Dry the bone blocks in an oven, drying conditions: 90°C, drying for 4 hours. Among them, the mass volume ratio of bone blocks to azeotropic mixture is 1:20.

[0056] 4. Calcination

[0057] Place the bone blocks flat on a stainless steel tray and then place them in a muffle furnace. Set the calcination parameters: 300°C for 15 hours. The heating process is not included in the calcination time, and the cooling process is to close the furnace door and cool down naturally.

[0058] 5. Drying

[0059] The calcined bone blocks were washed with ultrapure water and then placed in a forced air drying oven at 90°C for 4 hours.

[0060] 6. Sterilization

[0061] The dried bone blocks are packaged, encapsulated, and sterilized (cobalt-60 radiation sterilization, with an irradiation dose of 25 KGy).

[0062] Example 3

[0063] This embodiment relates to a method for preparing a novel block-shaped xenogeneic bone repair material, comprising the following steps:

[0064] 1. Materials taken:

[0065] Wearing work clothes, use a bone saw to cut the cancellous bone at the distal end of the bovine femoral epiphysis, use the bone saw to remove the accessory tissue around the flaky cancellous bone, and then cut it into bone blocks of (5-10)×(5-10)×(5-30) mm.

[0066] 2. Disinfection:

[0067] Place the cancellous bone block in a clean container, add 3 times the volume (mass volume ratio of the block bone to ethanol is 1:3) of 75% ethanol, soak for 30 minutes, drain, place the bone block in a clean container, weigh 15 times the volume (mass volume ratio of the block bone to purified water is 1:15) of purified water, add to the container. Perform ultrasonic cleaning 3 times, 10 minutes each time.

[0068] 3. Remove organic matter

[0069] Take the above disinfected bone block, put it in a flask, and then add 40% ethylenediamine, 30% ethylene glycol monomethyl ether, and 30% isobutyl alcohol to form an azeotropic mixture; Soxhlet extraction for 7 hours, changing the liquid once an hour; after completion, put the bone block in a clean container and weigh it, then add 20 times the amount (the mass volume ratio of the block bone to 75% ethanol is 1:20) of 75% ethanol, and ultrasonically clean it 3 times, 10 minutes each time. Then wash it under running water for 2 hours until it is neutral. Dry the bone block in an oven, drying conditions: 90°C, drying for 4 hours. Among them, the mass volume ratio of the bone block to the azeotropic mixture is 1:30.

[0070] 4. Calcination

[0071] Place the bone blocks flat on a stainless steel tray and then place them in a muffle furnace. Set the calcination parameters: calcination at 350℃ for 10h. The heating process is not included in the calcination time, and the cooling process is to close the furnace door and cool down naturally.

[0072] 5. Drying

[0073] The calcined bone blocks were washed with ultrapure water and then placed in a forced air drying oven at 90°C for 4 hours.

[0074] 6. Sterilization

[0075] The dried bone blocks are packaged, encapsulated, and sterilized (cobalt-60 radiation sterilization, with an irradiation dose of 25 KGy).

[0076] Cytotoxicity assay

[0077] The in vitro cytotoxicity test of oral restoration materials is one of the commonly used methods to detect the biosafety of materials. It is a biological evaluation and screening test of dental materials conducted using an in vitro tissue cell culture method to observe the effects of material extracts on cell growth, reproduction and morphology, and evaluate their in vitro cytotoxicity.

[0078] 1. Preparation of test samples

[0079] Under sterile operation, extract the sample with the extraction medium as described in the following groups. The state of the extract should not change before and after the extraction. The extract should be used for the experiment immediately.

[0080] Experimental group: Weigh the bone blocks, place them in the extraction medium to submerge them for adsorption, then take them out, drain them until there is no excess liquid on the surface, add 10 ml of the extraction medium, and shake them at 37°C and 60 rpm for 24 h.

[0081] Blank control group: directly measure 10 ml of the extraction medium and shake at 37°C and 60 rpm for 24 h.

[0082] Positive control group: Measure 1 ml of DMSO, add 9 ml of extraction medium, and shake at 37°C and 60 rpm for 24 h.

[0083] 2. Cell Preparation

[0084] Mouse fibroblasts were cultured in MEM medium containing antibiotics (penicillin 100 U / ml, streptomycin 100 μg / ml) and 10% fetal bovine serum at 37°C and 5% CO 2 Culture under saturated humidity. Use sterile operation during cell culture. When the cells grow to near confluence, use 0.25% trypsin to digest, collect the cells and adjust the cell concentration to 1×10 5 The following test was carried out with 100 μg / ml.

[0085] 3. Experimental steps

[0086] Add the above cell suspension to a 96-well plate, 100 μL per well, for a total of 1×10 4 cells / well, at 37°C, 5% CO 2 After culturing for 24 hours, the culture medium in the culture plate was discarded, and 100 μL of the extract was added to the plates (four concentration groups: 100%, 50%, 25% and 12.5%), negative control, blank control group and positive control group, 5 wells per group, and placed at 37°C, 5% CO 2 After 24 hours of culture, the cell culture plate was removed and morphological observation was performed first. Then the culture medium was discarded and 50 μL MTT was added to each well. The plate was placed in a 37°C, 5% CO 2 Incubate in a saturated humidity incubator for 2 h.

[0087] After the culture was completed, the liquid in the culture plate was discarded, 100 μL of isopropanol was added to each well, the plate was shaken and mixed, and the plate was placed in an ELISA reader and read at 570 nm (reference wavelength 650 nm). The relative cell survival rate of the experimental group and the positive control group was calculated by the OD value of the blank control group, and the blank control group was recorded as 100%.

[0088] Experimental results: The cell growth state was good through cell morphology observation and quantitative evaluation showed that the relative cell proliferation rate (%) was greater than 96%. According to the evaluation criteria, it was non-cytotoxic, which proved that this product had good cell compatibility and was safe and reliable.

[0089] Comparative Example 1

[0090] The comparative example relates to a method for preparing a block-shaped bone repair material, comprising the following steps:

[0091] 1. Materials taken:

[0092] Wearing work clothes, use a bone saw to cut the cancellous bone at the distal end of the femoral epiphysis of the cattle, and use the bone saw to remove the accessory tissue around the lamellar cancellous bone to form a bone block of (5-10)×(5-10)×(5-30)mm.

[0093] 2. Disinfection:

[0094] Place the cancellous bone block in a clean container, add 3 times the volume (mass volume ratio of the block bone to ethanol is 1:3) of 70% ethanol, soak for 30 minutes, drain, place the bone block in a clean container, weigh 15 times the volume (mass volume ratio of the block bone to purified water is 1:10) of purified water, add to the container, and perform ultrasonic cleaning 3 times, 10 minutes each time.

[0095] 3. Remove organic matter

[0096] Take the above disinfected bone blocks, put them into a flask, and then add 50% ethylenediamine, 20% ethylene glycol monomethyl ether, and 30% n-butanol to form an azeotropic mixture; Soxhlet extraction for 6 hours, changing the liquid once an hour; after completion, put the bone blocks into a clean container and weigh them, then add 20 times the amount (the mass volume ratio of block bone to 75% ethanol is 1:20) of 75% ethanol, and ultrasonically clean them 3 times, 10 minutes each time. Then wash them under running water for 2 hours until they are neutral. Dry the bone blocks in an oven, drying conditions: 90°C, drying for 4 hours. Among them, the mass volume ratio of bone blocks to azeotropic mixture is 1:20.

[0097] 4. Calcination

[0098] Place the bone blocks flat on a stainless steel tray and then place them in a muffle furnace. Set the calcination parameters to 230°C for 20 hours. The heating process is not included in the calcination time, and the cooling process is to close the furnace door and cool down naturally.

[0099] 5. Drying

[0100] The calcined bone blocks were washed with ultrapure water and then placed in a forced air drying oven at 90°C for 4 hours.

[0101] 6. Sterilization

[0102] The dried bone blocks are packaged, encapsulated, and sterilized (cobalt-60 radiation sterilization, with an irradiation dose of 25 KGy).

[0103] Comparative Example 2

[0104] This embodiment relates to a method for preparing a novel block-shaped xenogeneic bone repair material, comprising the following steps:

[0105] 1. Materials taken:

[0106] Wearing work clothes, use a bone saw to cut the cancellous bone at the distal end of the bovine femoral epiphysis, use the bone saw to remove the accessory tissue around the flaky cancellous bone, and then cut it into bone blocks of (5-10)×(5-10)×(5-30) mm.

[0107] 2. Disinfection:

[0108] Place the cancellous bone block in a clean container, add 5 times the volume (mass volume ratio of the block bone to ethanol is 1:5) of 75% ethanol, soak for 30 minutes, drain, place the bone block in a clean container, weigh 15 times the volume (mass volume ratio of the block bone to purified water is 1:15) of purified water, add to the container. Perform ultrasonic cleaning 3 times, 10 minutes each time.

[0109] 3. Remove organic matter

[0110] Take the above disinfected bone block, put it in a flask, and then add 40% ethylenediamine, 30% ethylene glycol monomethyl ether, and 30% isobutyl alcohol to form an azeotropic mixture; Soxhlet extraction for 7 hours, changing the liquid once an hour; after completion, put the bone block in a clean container and weigh it, then add 20 times the amount (the mass volume ratio of the block bone to 75% ethanol is 1:20) of 75% ethanol, and ultrasonically clean it 3 times, 10 minutes each time. Then wash it under running water for 2 hours until it is neutral. Dry the bone block in an oven, drying conditions: 90°C, drying for 4 hours. Among them, the mass volume ratio of the bone block to the azeotropic mixture is 1:30.

[0111] 4. Calcination

[0112] Place the bone blocks flat on a stainless steel tray and then place them in a muffle furnace. Set the calcination parameters: calcination at 380°C for 10 hours. The heating process is not included in the calcination time, and the cooling process is to close the furnace door and cool down naturally.

[0113] 5. Drying

[0114] The calcined bone blocks were washed with ultrapure water and then placed in a forced air drying oven at 90°C for 4 hours.

[0115] 6. Sterilization

[0116] The dried bone blocks are packaged, encapsulated, and sterilized (cobalt-60 radiation sterilization, with an irradiation dose of 25 KGy).

[0117] The performance of the bone repair materials prepared in Examples 1-3 of the present invention and Comparative Examples 1-2 are compared, as shown in the table.

[0118] Table 1

[0119] Compressive strength(MPa) Porosity (%) <![CDATA[Specific surface area m 2 / g]]> Micropore volume (ml / g) Example 1 4.84±0.15 82±3.4 88.07 0.3569 Example 2 4.71±0.10 80±4.1 90.7 0.4171 Example 3 4.77±0.13 81±4.7 91.8 0.4158 Comparative Example 1 1.68±0.16 65±6.8 57.2 0.0070 Comparative Example 2 6.14±0.22 66±3.6 71.4 0.3805

[0120] By comparing the test data of the above-mentioned embodiments 1-3 and comparative examples 1-2, it can be seen that the bone blocks treated by the method of the present invention have the following performance indicators: porosity (%), compressive strength (MPa), specific surface area (m 2 / g), micropore volume (ml / g) are better than those of comparative examples 1-2; in addition, see Figure 1-Figure 4 As shown; Figure 1This is a rendering of a bone block prepared by the method of the present invention, which has a natural porous three-dimensional spatial structure similar to human bones and a highly similar phase composition; Figure 2 This is a scanning electron microscope image of a bone block prepared by the method of the present invention. Figure 2 It can be seen that the bone block maintains the three-dimensional spatial structure of natural bone trabeculae and multi-level pores, with large pores of about 200-600μm, medium pores of 50-100μm, and micropores of ≤10μm. Figure 3 This is a diagram of the pore structure of the bone block prepared by the method of the present invention. The porosity of the bone block prepared by the method of the present invention is about 80%; Figure 4 The XRD spectrum of the bone block prepared by the method of the present invention is hydroxyapatite (HA, Ca 10 (PO 4 ) 6 (OH) 2 ), which matches the hydroxyapatite standard PDF card 09-432; while the characteristic peaks of synthetic hydroxyapatite are sharper and have higher diffraction intensity. Figure 5 is a cell morphology diagram of the cytotoxicity test involved in the present invention; Figure 6 It is the cell proliferation rate of the cytotoxicity test involved in the present invention. Through morphological observation, the relative cell survival rate (%) is quantitatively evaluated to be greater than 96%, which is non-cytotoxic, has good cell compatibility, and is safe and reliable.

[0121] The method involved in the present invention is to use ethylenediamine and ethylene glycol monomethyl ether, n-butanol, and isobutanol to form an azeotropic mixture, which not only shortens the process time, reduces the production of finished products, and improves efficiency. In addition, the natural structure of the bone is retained, ensuring that the crystallinity of the apatite crystals in the bone body is not significantly affected; it also avoids changes in structure and function caused by high-temperature calcination. In addition, compared with granular bone transplant materials, block bone transplants can have a good spatial support effect. The method involved in the present invention is an efficient defatting and deproteinizing method; the product prepared by this method not only has a natural porous three-dimensional spatial structure similar to human bones and a highly similar phase composition; it also has the advantages of high specific surface area, low immunogenicity, high safety, and good biocompatibility. The method involved in the present invention is a method for preparing a heterogeneous block bone transplant material, which overcomes the problems of spatial collapse and inability to maintain bone formation space in granular bone transplant materials.

[0122] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which will not affect the essence of the present invention.

Claims

1. A method for preparing a block-shaped xenogeneic bone repair material, characterized in that: The block-shaped xenogeneic bone repair material is prepared by the following steps: material selection, disinfection, defatting and deproteinization, calcination, drying, and sterilization; The specific steps of material selection are: (1) using a bone saw to cut the cancellous bone at the distal end of the femoral epiphysis of a bovine; (2) using a bone saw to remove the accessory tissues around the cancellous bone flakes; (3) cutting the bone strips into 2 cm long bone blocks, and the final product shape is a block bone of 10 mm×10 mm×20 mm; The specific steps of the disinfection are as follows: (1) placing the selected bone block in a clean container, adding 75% ethanol in a mass volume ratio of the bone block to the bone of 1: (2-5), soaking for 30 minutes, and draining; (2) placing the bone block in a clean container again, weighing purified water in a mass volume ratio of the bone block to the bone of 1: 15, and adding it to the container; (3) performing ultrasonic cleaning 3 times, each time for 10 minutes; The specific steps of defatting and deproteinizing are as follows: placing the detoxified block bone into a flask, and then adding an azeotropic mixture, wherein the azeotropic mixture is an azeotropic mixture of 10%-20% by mass of ethylene glycol monomethyl ether, 10%-30% by mass of n-butanol and 50%-80% by mass of ethylenediamine, or an azeotropic mixture of 10%-30% by mass of ethylene glycol monomethyl ether, 20%-30% by mass of isobutanol and 40%-70% by mass of ethylenediamine; The mass volume ratio of the bone block to the azeotropic mixture is 1:(10-30); The specific steps of the calcination are as follows: placing the bone block flat on a stainless steel tray, and sending it into a muffle furnace for calcination at 250-350° C. for 10-20 hours; The specific steps of drying are as follows: the calcined bone blocks are washed with ultrapure water and then dried in a blower at 90°C for 4 hours; The sterilization conditions are: cobalt-60 radiation sterilization, the irradiation dose is 25KGy; The block-shaped heterogeneous bone repair material is a three-dimensional structure composed of bone trabeculae and multi-level pores.

2. The method for preparing a block-shaped xenogeneic bone repair material according to claim 1, characterized in that: The multi-level pores include micropores, macropores and mesopores; wherein the macropores are 200-600 μm, the mesopores are 50-100 μm, and the micropores are ≤10 μm.