Hydrogenation catalyst containing modified alumina carrier, preparation method and application thereof, and hydrodenitrogenation method
By loading Group VIII and Group VIB metal elements and phosphorus elements on the modified alumina carrier, and designing the composition and pore size of the catalyst, the problem of easy deactivation of the hydrodenitrification catalyst in high-temperature reactions was solved, and the stability of the catalyst was achieved. Safety and high efficiency, suitable for industrial diesel hydrodenitrification.
Patent Information
- Application Number
- CN202111265085.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-10-28
AI Technical Summary
Existing hydrodenitrification catalysts are easily deactivated during high-temperature reactions and cannot effectively maintain activity and stability, affecting the operating cycle of the diesel hydrogenation unit.
A modified alumina carrier is used as the catalyst, and the pore size and composition of the catalyst are designed to maintain the activity and stability of the catalyst under high temperature conditions by loading Group VIII metal elements, Group VIB metal elements and phosphorus elements on it.
In high-temperature hydrodenitrification reactions, the modified alumina carrier catalyst maintains good activity and stability, improves reaction efficiency, is suitable for hydrodenitrification of industrial diesel, and has good industrial prospects.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to a hydrogenation catalyst containing a modified alumina carrier, a preparation method and application thereof, and a hydrogenation denitrogenation method. Background Art
[0002] The development of new energy is bound to have an impact on the demand for fossil fuels. The social demand for diesel may decrease to a certain extent. Refineries need to process diesel fractions reasonably to improve their economic value. Some diesel fractions have a high nitrogen content, and a stronger hydrodenitrogenation catalyst is required to remove the nitrogen before the diesel can be subsequently processed. The diesel hydrogenation process is a highly exothermic reaction, and the industrial diesel hydrogenation unit is an adiabatic reactor. Some reaction sections have a high reaction temperature, and high temperature will accelerate the deactivation of the catalyst. The use of high-stable hydrodenitrogenation catalysts in high-temperature zones is important for ensuring the operation cycle of the unit. Therefore, it is necessary to develop a high-stable diesel hydrodenitrogenation catalyst suitable for the high-temperature section to promote the comprehensive utilization of diesel fractions.
[0003] Patent application with application number 202010395989.6 discloses a hydrorefining catalyst and its preparation method and application. The catalyst includes 50-80wt% of a carrier and 20-50wt% of an active metal component. The carrier uses a composite oxide to regulate the interaction force between the active metal and the carrier in the catalyst, thereby increasing the concentration of active hydrogen species on the active metal surface and improving the hydrodesulfurization and hydrodenitrogenation reaction activity of the catalyst.
[0004] Patent application No. 201811455219.5 discloses a method for preparing a supported hydrogenation catalyst, wherein one or more of the group consisting of ethylenediaminetetramethylenephosphate, tetrabutylammonium fluoride and tartaric acid is used as an active metal positioning loading directing agent to position γ-Al 2 O 3 The carrier is contacted with a solution containing an active metal localized loading directing agent to prepare a catalyst, and the catalyst has high hydrodesulfurization, denitrification activity and aromatic hydrocarbon saturation activity.
[0005] Patent application No. 201710984468.2 discloses a bulk hydrorefining catalyst, comprising metal components of W, Ni and Mo. The steps of preparing the catalyst include: 1) conducting a gelling reaction of a mixed solution A containing Ni, W and Al, an organic additive and a precipitant in parallel, and aging the obtained slurry; 2) conducting a gelling reaction of a mixed solution B containing W and Al, MoO 3 The slurry and the precipitant are added to the aged slurry in parallel, and then aged; 3) drying, molding and other steps; the catalyst has high hydrodesulfurization and hydrodenitrogenation reaction activity, especially for treating diesel feedstock with high nitrogen and high sulfur content.
[0006] From the above, it can be seen that there is a need to study and develop diesel hydrodenitrogenation catalysts, but there is a lack of research and development of hydrodenitrogenation catalysts for high temperature environments. Summary of the invention
[0007] The purpose of the present invention is to overcome the problem that the hydrodenitrogenation catalyst in the prior art is easily deactivated during the high-temperature reaction process, and to provide a hydrogenation catalyst containing a modified alumina carrier, a preparation method and application thereof, and a hydrodenitrogenation method. The catalyst has good activity and stability, can maintain good activity and stability in the high-temperature hydrodenitrogenation reaction, has high reaction efficiency, and has good industrial prospects.
[0008] In order to achieve the above-mentioned object, the first aspect of the present invention provides a hydrogenation catalyst containing a modified alumina carrier, wherein the catalyst comprises a modified alumina carrier and a metal element of Group VIII and a metal element of Group VIB and a phosphorus element supported on the modified alumina carrier, wherein the pore size of the catalyst presents a unimodal pore distribution in the range of 8-20 nm; the catalyst composition is as follows: (Xi ai )·(Yi bi )·(Zi ci )·Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass of Xi in 1 gram of modified alumina support, Yi is a metal oxide of Group VIII, bi is the mass of Yi in 1 gram of modified alumina support, and Zi is P 2 O 5 , ci is equivalent to P in 1 g of modified alumina support 2 O 5 The mass of Sup refers to the modified alumina carrier in the catalyst, and its mass is 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.2-0.39nm, ρ Xi , Yi , Zi are Group VIB metal oxides, Group VIII metal oxides and P 2 O 5 The density of SA sup is the specific surface area of the modified alumina carrier; the modified alumina carrier contains a modified weak acid component.
[0009] It is worth noting that the ci here is relative to 1g of modified alumina support P 2 O 5 The quality of P 2 O 5Refers to P other than the modified weak acid component in the modified alumina carrier 2 O 5 , i.e., does not contain the modified weak acid component P in the modified alumina carrier 2 O 5 .
[0010] Preferably, the modified weak acid component is selected from at least one of B, P and Si elements.
[0011] Preferably, in the modified alumina carrier, the content of the modified weak acid component is 1-10 wt % calculated as oxide.
[0012] Preferably, in the modified alumina carrier, B 2 O 3 The content is 1.5-4% by weight, or P 2 O 5 The content is 2-6% by weight, or SiO 2 The content is 5-10% by weight.
[0013] The second aspect of the present invention provides a method for preparing a hydrogenation catalyst containing a modified alumina carrier as described in the first aspect, the method comprising: introducing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound and optionally an organic alcohol compound and / or a carboxylic acid compound containing -OH into the modified alumina carrier by an impregnation method, and then drying.
[0014] The third aspect of the present invention provides use of the hydrogenation catalyst containing the modified alumina carrier described in the first aspect in a hydrodenitrogenation reaction.
[0015] The fourth aspect of the present invention provides a hydrodenitrogenation method, which comprises: contacting the distillate oil with a catalyst under hydrodenitrogenation conditions, wherein the catalyst is the hydrogenation catalyst containing a modified alumina carrier as described in the first aspect.
[0016] The inventors of the present invention discovered during research that a modified alumina carrier is obtained by introducing a modified weak acid component into an alumina carrier to modify the alumina, and then the modified alumina carrier is used as a carrier of a hydrogenation catalyst containing the modified alumina carrier, and the composition of the catalyst is designed according to the above expression so that each component in the hydrogenation catalyst containing the modified alumina carrier satisfies the above expression. The hydrogenation catalyst containing the modified alumina carrier provided in this way is particularly suitable for high-temperature hydrodenitrogenation reaction. During the high-temperature hydrodenitrogenation reaction, the hydrogenation catalyst containing the modified alumina carrier maintains good activity and stability, can produce clean diesel more stably, has good industrial application prospects, and is worthy of large-scale promotion. DETAILED DESCRIPTION
[0017] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0018] A first aspect of the present invention provides a hydrogenation catalyst containing a modified alumina carrier, wherein the catalyst comprises a modified alumina carrier and a metal element of Group VIII and a metal element of Group VIB and a phosphorus element supported on the modified alumina carrier, wherein the pore size of the catalyst is in the range of 8-20 nm and presents a unimodal pore distribution;
[0019] Catalyst composition according to (Xi ai )·(Yi bi )·(Zi ci )·Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of modified alumina support Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of modified alumina support Yi, Zi is P 2 O 5 , ci is relative to 1 gram of modified alumina support P 2 O 5 The mass of Sup refers to the modified alumina carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.2-0.39nm, ρ Xi , Yi , Zi are Group VIB metal oxides, Group VIII metal oxides and P 2 O 5 The density of SA sup is the specific surface area of the modified alumina support;
[0020] The modified alumina carrier contains a modified weak acid component.
[0021] In the present invention, ρMoO 3 ,ρWO 3 ,ρNiO,ρCoO,ρP 2 O 5 According to 4.69g / cm 3 、 7.16g / cm 3 、6.67g / cm 3 、6.45g / cm3 and 2.39 g / cm 3 calculate.
[0022] It is worth noting that ci here is relative to 1 gram of modified alumina support, P 2 O 5 The quality of P 2 O 5 Refers to P other than the modified weak acid component in the modified alumina carrier 2 O 5 , i.e., does not contain the modified weak acid component P in the modified alumina carrier 2 O 5 .
[0023] In the present invention, the alumina carrier is modified by using a modified weak acid component to obtain a modified alumina carrier, and then the composition of the catalyst is limited by the above expression. On the one hand, the denitrification activity of the catalyst can be promoted, and on the other hand, the active metal elements are loaded on the modified alumina carrier so that the pore size of the hydrodenitrification catalyst is reasonable, the volumetric carbon capacity is increased, the stability of the catalyst is promoted, and the performance requirements of the hydrodenitrification catalyst in the high temperature section of the hydrodenitrification reaction are met.
[0024] In the present invention, there is no specific limitation on the type of modified weak acid component, as long as it can meet the performance requirements of the catalyst. Preferably, the modified weak acid component is selected from at least one of B, P and Si elements. The advantage of adopting this preferred embodiment is that the acidity of the carrier can be better improved, the hydrodenitrogenation effect of the catalyst can be increased, and the stability of the high temperature reaction can be promoted.
[0025] In the present invention, there is no specific limitation on the content of the modified weak acid component, as long as it can meet the performance requirements of the catalyst. Preferably, in the modified alumina carrier, the content of the modified weak acid component is 1-10 wt %, more preferably 2-8 wt %, calculated as oxide.
[0026] In the present invention, the weakly acidic component is provided by a compound containing a modified weakly acidic component. In a preferred embodiment, in the modified alumina carrier, B 2 O 3 The content is 1.5-4% by weight, or P 2 O 5 The content is 2-6% by weight, or SiO 2 The content is 5-8% by weight.
[0027] In the present invention, there is no specific restriction on the introduction method of the modified weak acid component, and conventional methods in the art are applicable to the present invention. For example, an impregnation method can be selected. In a preferred embodiment, the present invention adopts a co-impregnation method to introduce the modified weak acid component.
[0028] In the present invention, there is no particular restriction on the timing of introducing the modified weak acid component, which can be introduced during the preparation of the alumina support or after the preparation of the alumina support. Preferably, the following method can be adopted: the modified weak acid component is introduced after the preparation of the alumina support, and then calcined to obtain the modified alumina support.
[0029] In the present invention, when the modified weak acid component is introduced after the alumina carrier is prepared, the modified weak acid component is provided by a compound containing a weak acid component. Preferably, the compound containing a weak acid component is selected from at least one of boric acid, silica sol, phosphoric acid, hypophosphorous acid, ammonium phosphate and diammonium phosphate.
[0030] In the present invention, the specific conditions for calcination can be selected in a wide range. Preferably, the calcination temperature is 500-800°C and the calcination time is 2-10 hours.
[0031] In the present invention, when the modified weak acid component is introduced during the preparation of the alumina carrier, preferably, the compound containing the weak acid component can be directly added in the form of a precursor.
[0032] There is no specific limitation on the preparation method of the alumina carrier in the present invention. Conventional preparation methods in the art are applicable to the present invention and will not be described in detail herein.
[0033] In a preferred embodiment, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.26-0.39 nm. The use of this preferred embodiment can keep the catalyst pores relatively smooth, increase the volumetric carbon capacity of the catalyst, and promote the stability of the catalyst.
[0034] In a preferred embodiment, in the catalyst, the volume of pores with a pore size distribution of 2-6 nm accounts for no more than 5-15% of the total pore volume of the catalyst, and more preferably 6-10%.
[0035] In a preferred embodiment, the specific surface area of the catalyst is 165-210 m 2 / g, preferably 170-200m 2 / g.
[0036] In a preferred embodiment, the average pore size of the catalyst is 7-15 nm, preferably 8-15 nm.
[0037] In a preferred embodiment, the pore volume of the catalyst is 0.3-0.55 cm 3 / g, preferably 0.35-0.5cm 3 / g.
[0038] The present invention provides a catalyst with the above-mentioned specific composition and structure. The catalyst can maintain good activity and stability in the denitrification reaction in diesel, has excellent denitrification performance, and can efficiently produce clean diesel.
[0039] In the present invention, the specific surface area, pore volume, average pore diameter and pore distribution of the hydrogenation catalyst containing the modified alumina carrier are measured after the catalyst is calcined at 400 degrees for 3 hours.
[0040] In the present invention, the specific surface area, pore volume, average pore size and pore distribution of the catalyst are measured by low temperature nitrogen adsorption method (BET) (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990).
[0041] In the present invention, unless otherwise specified, pores of 8-20 nm refer to pores with a pore diameter greater than or equal to 8 nm and less than 20 nm.
[0042] In the present invention, alumina with specific physical properties is selected as a carrier precursor of modified alumina. Preferably, the water absorption rate of alumina in the modified alumina carrier is greater than 0.9 mL / g, and the specific surface area is greater than 260 m 2 / g, the average pore size is greater than 8nm, and further preferably, in the modified alumina carrier, the water absorption rate of alumina is 0.9-1.1mL / g, the specific surface area is 260-350m 2 / g, average pore size 8-15nm, pore distribution morphology is unimodal pore distribution. The purpose of adopting this preferred embodiment is to enable the catalyst to have a relatively wide pore structure, promote the contact between the reactants and the active components at high temperature, and enhance the hydrogenation and denitrification function of the catalyst.
[0043] In a preferred embodiment, in the alumina, the volume of pores with pore diameter distribution in the range of 2-6 nm accounts for no more than 10% of the total pore volume of the alumina, more preferably no more than 8%, and further 2-7%.
[0044] In a preferred embodiment, in the alumina, the volume of pores with pore diameter distribution in the range of 2-4 nm accounts for no more than 4%, preferably no more than 3% of the total pore volume of the alumina.
[0045] The use of the preferred alumina having the above-mentioned physicochemical parameters is more conducive to the improvement of catalyst hydrodenitrogenation and activity stability.
[0046] In the present invention, the Group VIII metal element includes but is not limited to at least one of Fe, Co and Ni, preferably Co and / or Ni.
[0047] In a preferred embodiment, the VIB Group metal element includes but is not limited to at least one of Cr, Mo and W, preferably Mo and / or W.
[0048] In the present invention, there is no specific restriction on the amount of the VIB group metal element and the phosphorus element in the catalyst, as long as the performance of the hydrogenation catalyst containing the alumina carrier is met. It should be noted that the phosphorus-containing compound here is the amount of phosphorus in 1 gram of the modified alumina carrier. 2 O 5 The quality of P 2 O 5 It refers to the modified weak acid component P in the modified alumina carrier. 2 O 5 Other P 2 O 5 , i.e., does not contain the modified weak acid component P in the modified alumina carrier 2 O 5 Preferably, the molar ratio of Zi / Xi in the catalyst is 0.05-0.45:1, preferably 0.2-0.38:1. This preferred embodiment can improve the solubility of the active metal component, maintain an appropriate amount of phosphate, and promote the dispersion of the active metal component.
[0049] In a preferred embodiment, the atomic concentration of the VIB group metal element in the catalyst on the surface of the modified alumina carrier is 2-5.5 atom / nm 2 , preferably 3-4.5atom / nm 2 .
[0050] In the present invention, the atomic concentration refers to the average atomic concentration of the VIB group element on the surface of the carrier, which is obtained by measuring the metal loading and the specific surface area of the carrier and then calculating. Specifically, it can be calculated by the following formula: (ai / M Xi )×N A / (1×SA sup ), where N A is Avogadro's constant, ai is the mass relative to 1 gram of modified alumina carrier Xi, M Xi is the molecular weight of Xi, SA sup is the specific surface area of the carrier. Using the atomic concentration within this range can ensure the formation of a moderate number of active centers, which can not only meet the needs of the reaction, but also provide enough space for the reaction, so as to achieve the purpose of promoting diffusion and reducing carbon deposition.
[0051] In the present invention, there is no specific restriction on the amount of the metal element of Group VIB in the catalyst. Preferably, the atomic ratio of the metal element of Group VIII to the total amount of the metal element of Group VIII and the metal element of Group VIB in the catalyst is 0.2-0.38, preferably 0.2-0.3. This preferred embodiment can better promote the synergistic effect between the metal element of Group VIB and the metal element of Group VIII, and meet the requirements of hydrodenitrogenation activity under high temperature conditions.
[0052] In this aspect, preferably, the catalyst further comprises one or more -OH-containing organic alcohol compounds and / or carboxylic acid compounds, and the molar ratio of the organic alcohol compounds and / or carboxylic acid compounds to the Group VIII metal elements is 1 to 4, preferably 2 to 4. The purpose of adopting this preferred embodiment is to ensure that the Group VIII metal elements have a higher dispersibility, weaken the interaction between the carrier and the metal, and promote the generation of more active phases.
[0053] In a preferred embodiment, the organic alcohol compound containing -OH can be at least one of a monohydric alcohol, a dihydric alcohol and a polyhydric alcohol. In a particularly preferred embodiment, the organic alcohol compound containing -OH is selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, amyl alcohol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol and trimethylolethane. In a more particularly preferred embodiment, the organic alcohol compound containing -OH is selected from at least one of glycerol, propanol and ethylene glycol.
[0054] In a preferred embodiment, the carboxylic acid compound is selected from one or more of formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid and tartaric acid, more preferably citric acid.
[0055] In a particularly preferred embodiment, the catalyst comprises one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol, trimethylolethane and / or formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid, tartaric acid.
[0056] In the present invention, there is no specific limitation on the size of the catalyst. Preferably, the equivalent diameter of the catalyst is 0.5-1.8 mm, more preferably 0.8-1.6 mm.
[0057] In the present invention, there is no specific limitation on the shape of the catalyst, and conventional catalyst shapes in the art are applicable to the present invention. Preferably, the catalyst is cylindrical, clover, four-leaf clover, honeycomb or other irregular shapes, more preferably cylindrical, clover or four-leaf clover.
[0058] The second aspect of the present invention provides a method for preparing the hydrogenation catalyst containing the modified alumina carrier according to the first aspect, the method comprising:
[0059] The Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound and optionally the -OH-containing organic alcohol compound and / or the carboxylic acid compound are introduced into the modified alumina carrier by an impregnation method, and then dried.
[0060] According to the method of the present invention, the "optionally containing -OH organic alcohol compounds and / or carboxylic acid compounds" means that -OH organic alcohol compounds and / or carboxylic acid compounds may be introduced into the modified alumina carrier, or may not be introduced. In the present invention, introduction is preferred.
[0061] According to the method of the present invention, the types of Group VIII metals, Group VIB metals, -OH-containing organic alcohol compounds, and carboxylic acid compounds have been described in the first aspect and will not be described again here.
[0062] According to the method of the present invention, preferably, the VIB Group metal precursor includes but is not limited to one or more of ammonium heptamolybdate, ammonium molybdate, ammonium phosphomolybdate, molybdenum oxide, ammonium metatungstate, ethylammonium metatungstate and tungsten oxide.
[0063] In a preferred embodiment, the Group VIII metal precursor includes, but is not limited to, one or more of cobalt nitrate, basic cobalt carbonate, cobalt acetate, cobalt oxide, nickel nitrate, basic nickel carbonate, nickel acetate and nickel oxide.
[0064] In a particularly preferred embodiment, the VIB Group metal and VIII Group metal precursors include but are not limited to one or more of ammonium heptamolybdate, ammonium molybdate, ammonium phosphomolybdate, molybdenum oxide, ammonium metatungstate, ethylammonium metatungstate, tungsten oxide, cobalt nitrate, basic cobalt carbonate, cobalt acetate, cobalt oxide, nickel nitrate, basic nickel carbonate, nickel acetate and nickel oxide.
[0065] In a preferred embodiment, the phosphorus-containing compound includes, but is not limited to, one or more of phosphoric acid, hypophosphorous acid, ammonium phosphate and diammonium phosphate.
[0066] In a preferred embodiment, the amount of the Group VIII metal precursor, the Group VIB metal precursor, and the phosphorus-containing compound is such that the catalyst obtained satisfies the above (ai / ρXi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value required.
[0067] According to the method of the present invention, there is no specific limitation on the impregnation method, and conventional impregnation methods in the art are applicable to the present invention. For example, it can be one of co-impregnation, step-by-step impregnation, saturated impregnation and supersaturated impregnation. In a preferred embodiment, co-impregnation is selected in the present invention. In a more preferred embodiment, the impregnation method comprises: impregnating the modified alumina carrier with an impregnation solution containing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and optionally an organic alcohol compound containing -OH and / or a carboxylic acid compound.
[0068] According to the method of the present invention, there is no specific limitation on the order of adding the Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound, and optionally the organic alcohol compound containing -OH and / or the carboxylic acid compound, as long as it is conducive to uniform mixing of the components. In a preferred embodiment, the Group VIII metal precursor, the Group VIB metal precursor, and the organic alcohol compound containing -OH and / or the carboxylic acid compound are added to an aqueous solution of the phosphorus-containing compound to prepare the impregnation solution. In the present invention, the order of adding the organic alcohol compound containing -OH and / or the carboxylic acid compound, the phosphorus-containing compound, and the metal precursor can also be interchanged.
[0069] According to the method of the present invention, the catalyst has the structure and composition of the first aspect according to the physical properties of the modified alumina carrier and the feed amount of each material. The present invention has no particular limitation on this. In order to facilitate the understanding of the technical solution of the present invention, an exemplary description is now provided to embody the preparation method of the present invention, and the method of the present invention includes but is not limited to this. For example, a hydrogenation catalyst containing a modified alumina carrier can be prepared by the following preparation method: (1) Determine the feed amount of the VIB group metal precursor per gram of the modified alumina carrier according to the surface atomic concentration of the VIB group metal element and the specific surface area of the modified alumina carrier; (2) Determine the feed amount of the VIII group metal precursor per gram of the modified alumina carrier according to the atomic ratio of the VIII group metal element to the total amount of the VIII group metal element and the VIB group metal element; (3) Determine the feed amount of the VIII group metal precursor per gram of the modified alumina carrier according to (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of P 2 O 5(4) calculating the feeding amount of the -OH-containing organic alcohol compound and / or the carboxylic acid compound according to the molar ratio of the -OH-containing organic alcohol compound and / or the carboxylic acid compound to the Group VIII metal element; (5) according to the feeding amounts of the above-mentioned Group VIB metal precursor, Group VIII metal precursor, the phosphorus-containing compound and the -OH-containing organic alcohol compound and / or the carboxylic acid compound, the modified alumina carrier is impregnated with the impregnation liquid by the pore saturation impregnation method, and then dried. Specifically, a phosphorus-containing compound is first dissolved in water to obtain a phosphorus-containing aqueous solution, and then an organic alcohol compound and / or a carboxylic acid compound containing -OH, a VIB group metal precursor and a VIII group metal precursor are added, and the mixture is stirred under heating until it is completely dissolved, and the temperature is kept constant to obtain an impregnation solution; (6) the water absorption rate of the modified alumina carrier is measured, and the liquid absorption rate of the modified alumina carrier is calculated according to the formula of water absorption rate of the modified alumina carrier-0.1; (7) according to the liquid absorption rate of the modified alumina carrier, the impregnation solution is adjusted to a corresponding volume (liquid absorption rate of the modified alumina carrier×mass of the carrier), and the impregnation solution and a corresponding mass of the modified alumina carrier are evenly mixed and allowed to stand, and then dried to prepare a hydrogenation catalyst containing the modified alumina carrier.
[0070] In the present invention, the drying conditions have a wide range of selections. Preferably, the drying conditions include: a temperature of 80-200° C. and a time of 1-10 h.
[0071] The third aspect of the present invention provides use of the hydrogenation catalyst containing the modified alumina carrier described in the first aspect in a hydrodenitrogenation reaction.
[0072] The fourth aspect of the present invention provides a hydrodenitrogenation method, which comprises: contacting the distillate oil with a catalyst under hydrodenitrogenation conditions, wherein the catalyst is the hydrogenation catalyst containing a modified alumina carrier as described in the first aspect.
[0073] In a preferred embodiment, the hydrodenitrogenation conditions include: pressure of 3-14 MPa, temperature of 350-410°C, volume space velocity of 0.5-10 hours -1 , the volume ratio of hydrogen to oil is 200-1000:1; the preferred temperature is 360-400℃.
[0074] In a particularly preferred case, the temperature of the hydrodenitrogenation reaction of the hydrogenation catalyst containing an alumina carrier is 370-390°C. The hydrogenation catalyst containing a modified alumina carrier of the present invention is particularly suitable for hydrodenitrogenation reactions in high temperature sections. In the hydrodenitrogenation reaction, the hydrogenation catalyst containing a modified alumina carrier can maintain good activity, is not easily deactivated, and greatly improves the reaction efficiency.
[0075] According to the method provided by the present invention, preferably, before the contacting, the distillate oil is first subjected to a first contact reaction with a first hydrogenation catalyst, and then subjected to a contact reaction with the hydrogenation catalyst containing a modified alumina carrier provided by the present invention.
[0076] Preferably, the packing volume ratio of the first hydrogenation catalyst and the hydrogenation catalyst containing the modified alumina carrier provided by the present invention is 1:2-4:1.
[0077] The first hydrogenation catalyst may be any hydrodenitrogenation catalyst conventionally used in the art, and may be commercially available or prepared by the user, and the present invention will not elaborate on this.
[0078] Preferably, the conditions of the first contact reaction include: pressure of 3-14 MPa, temperature of 300-380°C, volume space velocity of 1-6 hours -1 , the volume ratio of hydrogen to oil is 200-1200:1.
[0079] In the present invention, the hydrodenitrogenation reaction of the hydrogenation catalyst containing the modified alumina carrier is measured on a high-pressure small-scale reactor, the upper bed layer is filled with industrial catalyst, and the lower bed layer is filled with the hydrogenation catalyst containing the modified alumina carrier described in the first aspect of the present invention.
[0080] In a preferred embodiment, the sulfur content in the distillate oil is 3000-30000 ppm, and the nitrogen content is 50-3000 ppm.
[0081] In a preferred case, the catalyst needs to be converted from an oxidized catalyst to a sulfurized catalyst by sulfurization before use. In the present invention, there is no specific limitation on the sulfurization method, and conventional sulfurization methods in the art are applicable to the present invention. Preferably, for example, it can be one of dry sulfurization and wet sulfurization. There is no particular limitation on the type of the vulcanizing agent, and those skilled in the art can select it according to conventional schemes in the art.
[0082] In a preferred embodiment, the vulcanization conditions include: vulcanization temperature of 280-420°C, heating rate of 5-60°C / hour, time of 10-48h, pressure of 0.1-15MPa, volume space velocity of 0.5-20h -1 , the volume ratio of hydrogen to oil is 100-2000:1.
[0083] The present invention will be described in detail below by way of examples. In the following examples, the hydrodesulfurization performance of the catalyst was measured on a high-pressure small reactor, with 6 mL of an industrial catalyst loaded on the upper bed, the composition of which was 4.3% by weight of NiO, 27% by weight of MoO 3, 68.7 wt% alumina, 10 mL of the catalyst of the present invention is loaded in the lower bed, and the oxidized catalyst is directly converted into the sulfided catalyst by the programmed temperature rise sulfidation method. The sulfidation conditions are: the sulfidation pressure is 6.4 MPa, the sulfiding oil is CS 2 2% by weight kerosene, volume space velocity 2 hours -1 , the hydrogen-to-oil volume ratio is 300v / v, first keep the temperature at 230℃ / h for 6h, then increase the temperature to 360℃ for sulfidation for 8h, and the heating rate of each stage is 10℃ / h. After sulfidation, switch the reaction raw materials for hydrodesulfurization activity test. The reaction raw materials are high nitrogen distillate oil with a sulfur content of 4000ppm and a nitrogen content of 1154ppm. The test conditions are: pressure of 10MPa, volume space velocity of 1.5h -1 , hydrogen oil volume ratio of 800v / v, reaction temperature of 370℃. After the reaction was stable for 2 days, the product properties were analyzed. The catalyst was deactivated at high temperature and high space velocity (reaction temperature of 390℃, volume space velocity of 3.0h -1 , reaction time 3 days), at a pressure of 10.0 MPa and a volume space velocity of 1.5 hours -1 The test was carried out under the conditions of a hydrogen-to-oil volume ratio of 800 v / v and a reaction temperature of 370°C, and the nitrogen content in the product was analyzed to compare the stability of the catalyst.
[0084] The composition of the catalyst is calculated based on the feed amount. The pore distribution, pore size and pore volume of 2-100 nm in the catalyst and the carrier are determined by low temperature nitrogen adsorption method (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). The nitrogen mass fraction in the product is analyzed using a sulfur-nitrogen analyzer (produced by Thermo Fisher, model TN / TS3000).
[0085] Example 1
[0086] A γ-alumina carrier was selected, and 2 wt% B was introduced by impregnation after the carrier was prepared. 2 O 3 The modified alumina carrier has a water absorption rate of 1.02 mL / g and a specific surface area of 271 m 2 / g, the average pore size is 12.5nm, the pore volume with a pore size of 2-6nm accounts for 7.4% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3.2% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0087] A certain amount of MoO 3, basic nickel carbonate, and glycerol were added to the aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0088] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0089] The atomic concentration of Mo in the catalyst is 4.3atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P 2 O 5 / MoO 3 The molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.33 nm, and the molar ratio of glycerol to Ni is 2.
[0090] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 188m 2 / g, pore volume 0.43cm 3 / g, the average pore size is 9.1nm, and the pore size of the catalyst is distributed in a single peak in the range of 8-20nm. After the catalyst is sulfurized and tested for reaction, the nitrogen content in the product is 1.5ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the product is 8.6ppm.
[0091] Example 2
[0092] A γ-alumina carrier was selected, and 4 wt% of P was introduced by impregnation after the carrier was prepared. 2 O 5 The modified alumina carrier has a water absorption rate of 0.96 mL / g and a specific surface area of 269 m 2 / g, the average pore size is 11.9nm, the pore volume with a pore size of 2-6nm accounts for 7.5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3.6% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0093] A certain amount of MoO 3, basic nickel carbonate, and glycerol were added to the aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0094] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0095] The atomic concentration of Mo in the catalyst is 3.2atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.3, P 2 O 5 / MoO 3 The molar ratio is 0.3, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.283nm, and the molar ratio of glycerol to Ni is 4.
[0096] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 205m 2 / g, pore volume 0.48cm 3 / g, the average pore size is 9.4nm, and the pore size of the catalyst is unimodal in the range of 8-20nm. After the catalyst is sulfurized and tested for reaction, the nitrogen content in the product is 1.8ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the product is 9.0ppm.
[0097] Example 3
[0098] A γ-alumina carrier was selected, and 6 wt% SiO was introduced by impregnation after the carrier was prepared. 2 The modified alumina carrier has a water absorption rate of 0.95 mL / g and a specific surface area of 275 m 2 / g, the average pore size is 9.8nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0099] A certain amount of MoO 3 , basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 95°C for 2 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0100] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0101] The atomic concentration of Mo in the catalyst is 3.6atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.28, P 2 O 5 / MoO 3 The molar ratio is 0.25, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbonyl group is 0.298 nm, and the molar ratio of glycerol to Ni is 3.
[0102] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 198m 2 / g, pore volume 0.45cm 3 / g, the average pore size is 9.1nm, and the pore size of the catalyst is distributed in a single peak in the range of 8-20nm. After the catalyst is sulfurized and tested for reaction, the nitrogen content in the product is 2.1ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the product is 9.9ppm.
[0103] Example 4
[0104] A γ-alumina carrier was selected, and 2 wt% P was introduced by impregnation after the carrier was prepared. 2 O 5 The modified alumina carrier has a water absorption rate of 0.97 mL / g and a specific surface area of 265 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 6.5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 2% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0105] A certain amount of ammonium metatungstate, basic nickel carbonate and citric acid were added to the aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 130°C for 3 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0106] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0107] The atomic concentration of W in the catalyst is 4atom / nm 2 , Ni / (Ni+W) atomic ratio is 0.3, P2 O 5 / WO 3 The molar ratio is 0.35, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.385 nm, and the molar ratio of citric acid to Ni is 2.
[0108] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 168m 2 / g, pore volume 0.39cm 3 / g, the average pore size is 9.3nm, and the pore size of the catalyst is distributed in a single peak in the range of 8-20nm. After the catalyst is sulfurized and tested for reaction, the sulfur content in the product is 3.5ppm and the nitrogen content is 1.1ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the product is 7.9ppm.
[0109] Example 5
[0110] The γ-alumina carrier was selected and 8 wt% SiO was introduced during the carrier preparation process. 2 The modified alumina carrier has a water absorption rate of 0.92 mL / g and a specific surface area of 258 m 2 / g, the average pore size is 9.8nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0111] A certain amount of MoO 3 , basic nickel carbonate, and citric acid were added to the aqueous solution containing phosphoric acid, heated and stirred at 90°C for 2 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0112] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0113] The atomic concentration of Mo in the catalyst is 3.8atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.32, P 2 O 5 / MoO 3 The molar ratio is 0.3, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SAsup is 0.34 nm, and the molar ratio of citric acid to Ni is 2.
[0114] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst was 183m 2 / g, pore volume 0.47cm 3 / g, the average pore size is 10.3nm, and the pore size of the catalyst is unimodal in the range of 8-20nm. After the catalyst is sulfurized and tested for reaction, the nitrogen content in the product is 1.6ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the product is 8.8pm.
[0115] Example 6
[0116] The γ-alumina carrier was selected and 1.5 wt% B was introduced during the carrier preparation process. 2 O 3 The modified alumina carrier has a water absorption rate of 0.96 mL / g and a specific surface area of 274 m 2 / g, the average pore size is 11.9nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0117] A certain amount of MoO 3 , basic nickel carbonate, and citric acid were added to the aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 160°C for 3 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0118] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0119] The atomic concentration of Mo in the catalyst is 4.0atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.2, P 2 O 5 / MoO 3 The molar ratio is 0.25, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.32 nm, and the molar ratio of citric acid to Ni is 2.
[0120] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 188m2 / g, pore volume 0.47cm 3 / g, the average pore size is 10.0nm, and the pore size of the catalyst is distributed in a single peak in the range of 8-20nm. After the catalyst is sulfurized and tested for reaction, the nitrogen content in the product is 2.2ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the product is 10.5ppm.
[0121] Comparative Example 1
[0122] The same modified alumina carrier as in Example 1 was selected to prepare the catalyst. A certain amount of MoO 3 , basic nickel carbonate, and glycerol were added to the aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0123] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0124] The atomic concentration of Mo in the catalyst is 1.9atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.19, P 2 O 5 / MoO 3 The molar ratio is 0.3, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.161 nm, and the molar ratio of glycerol to Ni is 2.
[0125] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 233m 2 / g, pore volume 0.6cm 3 / g, the average pore size is 10.3nm, and the pore size of the catalyst is unimodal in the range of 8-20nm. After the catalyst is sulfurized and tested for reaction, the nitrogen content in the product is 7.5ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the product is 30.5ppm.
[0126] Comparative Example 2
[0127] The same modified alumina carrier as in Example 1 was selected to prepare the catalyst. A certain amount of MoO 3, basic nickel carbonate, and glycerol were added to the aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0128] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0129] The atomic concentration of Mo in the catalyst is 2.3atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.21, P 2 O 5 / MoO 3 The molar ratio is 0.22, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.178nm, and the atomic ratio of propylene glycol to Ni is 2.
[0130] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 225m 2 / g, pore volume 0.54cm 3 / g, the average pore size is 9.6nm, and the pore size of the catalyst is distributed in a single peak in the range of 8-20nm. After the catalyst is sulfurized and reacted, the nitrogen content in the product is 10.4ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the product is 35.6ppm.
[0131] It can be seen from the examples and comparative examples that the present invention has good inventive effects, and the prepared catalyst has high stability and activity under high temperature reaction conditions when placed in the lower bed, and has good industrial application prospects.
[0132] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A hydrogenation catalyst containing a modified alumina carrier, wherein: The catalyst comprises a modified alumina carrier and a metal element of Group VIII and a metal element of Group VIB and a phosphorus element supported on the modified alumina carrier, wherein the pore size of the catalyst is in the range of 8-20 nm and presents a unimodal pore distribution; Catalyst composition according to (Xi ai )•(Yi bi )•(Zi ci )•Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of the modified alumina carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of the modified alumina carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of the modified alumina carrier P2O5, Sup refers to the modified alumina carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.2-0.39nm, ρ Xi , Yi , Zi are the densities of Group VIB metal oxides, Group VIII metal oxides and P2O5, SA sup is the specific surface area of the modified alumina support; The modified alumina carrier contains a modified weak acid component; The modified weak acid component is selected from at least one of B, P and Si elements; In the modified alumina carrier, the content of the modified weak acid component is 1-10% by weight, calculated as oxide; In the catalyst, the volume of pores with a pore size distribution of 2-6 nm accounts for 5-15% of the total pore volume of the catalyst; The specific surface area of the catalyst is 165-210m 2 / g; The average pore size of the catalyst is 7-15 nm; The pore volume of the catalyst is 0.3-0.55 cm 3 / g.
2. The hydrogenation catalyst containing a modified alumina carrier according to claim 1, wherein In the modified alumina carrier, the B2O3 content is 1.5-4% by weight, or the P2O5 content is 2-6% by weight, or the SiO2 content is 5-8% by weight.
3. The hydrogenation catalyst containing a modified alumina carrier according to claim 1 or 2, wherein (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value is 0.26-0.39nm.
4. The hydrogenation catalyst containing a modified alumina carrier according to claim 1 or 2, wherein In the catalyst, the volume of pores with pore diameter distribution in the range of 2-6 nm accounts for 6-10% of the total pore volume of the catalyst.
5. The hydrogenation catalyst containing a modified alumina carrier according to claim 1 or 2, wherein The average pore size of the catalyst is 8-15 nm.
6. The hydrogenation catalyst containing a modified alumina carrier according to claim 1 or 2, wherein: The pore volume of the catalyst is 0.35-0.5 cm 3 / g.
7. The hydrogenation catalyst containing a modified alumina carrier according to claim 1 or 2, wherein: The water absorption rate of the modified alumina carrier is greater than 0.9 mL / g, and the specific surface area is greater than 260 m 2 / g, the average pore size is greater than 8nm, and the pore distribution morphology is a unimodal pore distribution.
8. The hydrogenation catalyst containing a modified alumina carrier according to claim 1 or 2, wherein: In the modified alumina carrier, the volume of pores with a pore size distribution of 2-6 nm accounts for no more than 10% of the total pore volume of the modified alumina carrier.
9. The hydrogenation catalyst containing a modified alumina carrier according to claim 8, wherein In the modified alumina carrier, the volume of pores with a pore size distribution of 2-6 nm accounts for no more than 8% of the total pore volume of the modified alumina carrier.
10. The hydrogenation catalyst containing a modified alumina carrier according to claim 1 or 2, wherein: In the modified alumina carrier, the volume of pores with a pore size distribution of 2-4 nm accounts for no more than 4% of the total pore volume of the modified alumina carrier.
11. The hydrogenation catalyst containing a modified alumina carrier according to claim 10, wherein: In the modified alumina carrier, the volume of pores with a pore size distribution of 2-4 nm accounts for no more than 3% of the total pore volume of the modified alumina carrier.
12. The hydrogenation catalyst containing a modified alumina carrier according to claim 1 or 2, wherein: The molar ratio of Zi / Xi in the catalyst is 0.05-0.45:
1.
13. The hydrogenation catalyst containing a modified alumina carrier according to claim 12, wherein: The molar ratio of Zi / Xi in the catalyst is 0.2-0.38:
1.
14. The hydrogenation catalyst containing a modified alumina carrier according to claim 1 or 2, wherein:The atomic concentration of the VIB group metal elements in the catalyst on the surface of the modified alumina carrier is 2-5.5atom / nm 2 .
15. The hydrogenation catalyst containing a modified alumina carrier according to claim 14, wherein The atomic concentration of the VIB group metal elements in the catalyst on the surface of the modified alumina carrier is 3-4.5atom / nm 2 .
16. The hydrogenation catalyst containing a modified alumina carrier according to claim 1 or 2, wherein: The atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the catalyst is 0.2-0.
38.
17. The hydrogenation catalyst containing a modified alumina carrier according to claim 16, wherein: The atomic ratio of the metal element of Group VIII to the total amount of the metal element of Group VIII and the metal element of Group VIB in the catalyst is 0.2-0.
3.
18. The hydrogenation catalyst containing a modified alumina carrier according to claim 1 or 2, wherein: The catalyst further comprises one or more organic alcohol compounds and / or carboxylic acid compounds containing -OH, and the molar ratio of the organic alcohol compounds and / or carboxylic acid compounds containing -OH to the metal element of Group VIII is 1-4.
19. The hydrogenation catalyst containing a modified alumina carrier according to claim 18, wherein The molar ratio of the -OH-containing organic alcohol compound and / or carboxylic acid compound to the Group VIII metal element is 2-4.
20. The hydrogenation catalyst containing a modified alumina carrier according to claim 1 or 2, wherein: The catalyst is in the shape of a cylinder, a three-leaf clover, a four-leaf clover, a butterfly, a honeycomb or other irregular shapes.
21. The hydrogenation catalyst containing a modified alumina carrier according to claim 1 or 2, wherein: The equivalent diameter of the catalyst is 0.5-1.8 mm.
22. The hydrogenation catalyst containing a modified alumina carrier according to claim 1 or 2, wherein: The equivalent diameter of the catalyst is 0.8-1.6 mm.
23. A method for preparing a hydrogenation catalyst containing a modified alumina carrier according to any one of claims 1 to 22, the method comprising: The Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound and optionally the -OH-containing organic alcohol compound and / or the carboxylic acid compound are introduced into the modified alumina carrier by an impregnation method, and then dried.
24. The preparation method according to claim 23, wherein: The impregnation method comprises: impregnating the modified alumina carrier with an impregnation solution containing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and optionally an organic alcohol compound containing -OH and / or a carboxylic acid compound.
25. The preparation method according to claim 24, wherein: The -OH-containing organic alcohol compound and / or carboxylic acid compound, Group VIII metal precursor, and Group VIB metal precursor are added to an aqueous solution of a phosphorus-containing compound to provide the impregnation solution.
26. The preparation method according to claim 23, wherein The drying conditions include: temperature of 80-200° C. and time of 1-10 h.
27. Use of the hydrogenation catalyst containing the modified alumina carrier as described in any one of claims 1 to 22 in a hydrodenitrogenation reaction.
28. A hydrodenitrogenation method, the method comprising: Under hydrodenitrogenation conditions, the distillate oil is contacted with the catalyst for reaction, wherein the catalyst is the hydrogenation catalyst containing a modified alumina carrier as claimed in any one of claims 1 to 22.
29. The hydrodenitrogenation method according to claim 28, wherein: The conditions of the hydrodenitrogenation include: pressure of 3-14 MPa, temperature of 350-410°C, volume space velocity of 0.5-10 hours -1 , the volume ratio of hydrogen to oil is 200-1000:
1.