Leakage repairing material for calcium carbide furnace water cooling equipment, preparation method thereof and leakage repairing method
By using mixed materials of orchid, coke and electrode paste particles, the leakage points of the water-cooling equipment of the calcium carbide furnace is quickly repaired, and the problem of time-consuming traditional welding and repair methods is solved, the equipment operation efficiency and lime utilization rate are improved, and safety and environmental risks are reduced.
Patent Information
- Application Number
- CN202211627634.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-16
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-16
AI Technical Summary
When the sealed calcium carbide furnace water cooling equipment is operated in a high temperature environment, the central furnace cover, furnace cover and water-cooled sealing sleeve leak, most of the leakage points are small and dense. The traditional welding and repair method is difficult to repair leaks and takes a long time, which leads to power outages in the equipment and affects calcium carbide. Yield.
The mixture of orchid, coke and electrode paste particles is used as the leak repair material. By detecting the size and location of the leak point, the leak repair material is poured into the water inlet pipe using asbestos rubber pipeline to quickly repair the leak point, and combined with compressed air to clear the blockage, simplifying the operation.
It reduces repair time, improves equipment operation rate, reduces furnace temperature loss, reduces the burden on lime powdering and purification system of the material surface, improves lime utilization rate, and avoids safety and environmental protection issues.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of chemical smelting, and in particular relates to a method for repairing leakage of water cooling equipment of a calcium carbide furnace. Background Art
[0002] The closed calcium carbide furnace smelting uses the high temperature generated by the electric arc to melt the raw materials and then react to form calcium carbide. The furnace cover, flue, electrode shield and other equipment of the closed calcium carbide furnace are welded with stainless steel plates. The welding structure is a double-layer jacket structure, and circulating cooling water is passed into the jacket to cool the equipment.
[0003] Calcium carbide furnace equipment operates in a high-temperature environment for a long time, and the metal is prone to plastic changes and stress relaxation. In the case of abnormal production and insulation damage, it may also cause short circuit perforation of the equipment. The main vulnerable equipment is the contact element, bottom ring, protective screen, center furnace cover, furnace cover, water-cooled sealing sleeve, etc. When repairing the contact element, bottom ring, and protective screen, the electrode can be lifted out of the furnace cover, which is relatively easy to operate. However, when the center furnace cover, furnace cover, and water-cooled sealing sleeve leak, the material column needs to be disassembled to repair the leak from inside the furnace, which is difficult to repair, dangerous, and time-consuming to repair.
[0004] If the cooling circulating water leaks into the calcium carbide furnace, the lime on the material surface will be powdered by water, and the powdered lime will be pumped away by the purification system, resulting in waste of raw materials and inaccurate ratio of entering the furnace. Large leakage can also cause the furnace surface temperature to drop, the material surface air permeability to be poor, the furnace pressure to fluctuate greatly, the furnace surface to cross the fire, and the furnace cover equipment to burn. Equipment leakage is one of the main reasons for the power outage of the calcium carbide furnace. Reducing or solving the problem of water leakage in the calcium carbide furnace is the key to stabilizing the furnace condition and increasing the output of calcium carbide.
[0005] The inventors found in actual use that these prior arts have at least the following technical problems:
[0006] According to the actual operation of the closed calcium carbide furnace, it was found that when the central furnace cover, furnace cover, and water-cooled sealing sleeve were leaking, most of the leakage points were small and dense. The traditional welding repair method was difficult and time-consuming. Summary of the invention
[0007] In order to overcome the above-mentioned deficiencies, the inventors of the present invention have continuously reformed and innovated through long-term exploration and attempts, multiple experiments and efforts, and proposed a leak-repairing material for calcium carbide furnace water-cooling equipment, its production method and leak-repairing method, which can solve the problems of high difficulty and long time spent on leak repair by using traditional welding repair methods.
[0008] To achieve the above purpose, the technical solution adopted by the present invention is: to provide a leak-proof material suitable for calcium carbide furnace water cooling equipment, which includes one or a mixture of blue coke, coke and electrode paste particles.
[0009] According to the leak-proof material suitable for calcium carbide furnace water cooling equipment described in the present invention, a further preferred technical solution is: the particle size of the blue coke, coke and electrode paste particles is 1-3mm.
[0010] According to the leak-proof material suitable for calcium carbide furnace water-cooling equipment described in the present invention, a further preferred technical solution is: the ratio of the blue coke, coke and electrode paste particles is 2:2:1.
[0011] Provided is a method for making a leak-proof material, comprising the following steps: selecting blue charcoal, coke and electrode paste particles; drying the blue charcoal, coke and electrode paste particles; and uniformly mixing the dried blue charcoal, coke and electrode paste particles.
[0012] According to the method for making a leak-proof material described in the present invention, a further preferred technical solution is: selecting blue charcoal, coke and electrode paste particles; drying the blue charcoal, coke and electrode paste particles; and uniformly mixing the dried blue charcoal, coke and electrode paste particles.
[0013] A method for repairing leaks in water-cooling equipment of a calcium carbide furnace comprises the following steps: a step of detecting the size and position of a leak: shutting down the calcium carbide furnace, checking the leak of the calcium carbide furnace, and determining the size and position of the leak; a step of repairing the leak: when the size of the leak meets a preset size and the position of the leak meets a preset position, shutting off the water inlet, removing the water inlet pipe of the leaking equipment, pouring leak repairing materials from the water inlet into the pipe of the leaking equipment, reinstalling the water inlet pipe, and then opening the water inlet.
[0014] According to the method for repairing leaks in water-cooling equipment of a calcium carbide furnace described in the present invention, a further preferred technical solution is: the preset size of the leak point is that the aperture of a single leak point is less than 3 mm, and the preset position of the leak point is the furnace cover, the center furnace cover and the water-cooling jacket equipment.
[0015] According to the method for repairing leaks in water-cooling equipment of a calcium carbide furnace described in the present invention, a further preferred technical solution is: after removing the water inlet pipe, an asbestos rubber pipe is connected at the water inlet, and the leak repairing material is poured in through the asbestos rubber pipe.
[0016] According to the method for repairing leaks in water-cooling equipment of a calcium carbide furnace described in the present invention, a further preferred technical solution is: after reinstalling the water inlet pipe, slowly open the water inlet.
[0017] According to the method for repairing leaks in water-cooling equipment for a calcium carbide furnace described in the present invention, a further preferred technical solution is that it also includes a clearing step: when the pipeline of the leaking equipment is blocked, the compressed air pipeline is connected to the water inlet and outlet of the leaking equipment.
[0018] Compared with the prior art, the technical solution of the present invention has the following advantages / benefits:
[0019] The repair method used in the present invention does not need to circulate all the water in the calcium carbide furnace, which saves time. The leak repair material is introduced to repair the leaking points at different positions of the leaking equipment according to the different densities of the components of the leak repair material. The operation is simple and it is not easy to miss.
[0020] The leak repair material of the present invention is used to quickly repair the furnace cover, center furnace cover, and water cooling jacket of the electric furnace. It takes about 15 minutes each time. The traditional welding leak repair takes about 60 minutes to treat a single leak. Each leak point is saved by 45 minutes, and the daily output of calcium carbide is indirectly increased by 6.5 tons, the time for power outage repair equipment is reduced, the equipment operation rate is greatly increased, and the furnace temperature loss is reduced. The amount of water leakage in the furnace is reduced, and the safety and environmental protection problems caused by large material collapse are avoided. The lime powder on the material surface is reduced and is sucked away by the purification system, and the lime utilization rate is improved. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. Therefore, the detailed description of the embodiments of the present invention provided below is not intended to limit the scope of the claimed invention, but merely represents the selected embodiments of the present invention.
[0022] Example:
[0023] A method for repairing leakage of water cooling equipment of calcium carbide furnace comprises the following steps:
[0024] Water leakage judgment steps:
[0025] When the hydrogen content in the calcium carbide furnace suddenly increases, the furnace pressure is difficult to control, the material surface temperature decreases, and the single-phase electrode drops rapidly, it is judged that there is a water leak in the calcium carbide furnace.
[0026] Steps for detecting the size and location of leaks:
[0027] Shut down the calcium carbide furnace, quickly check the leakage point of the calcium carbide furnace, and determine the size and location of the leakage point;
[0028] Leak repair steps:
[0029] When the aperture of a single leak is less than 3 mm, and the leak is located at the furnace cover, center furnace cover and water-cooling jacket equipment, find the water inlet pipe of the leaking equipment, shut off the water inlet, remove the water inlet pipe of the leaking equipment, and then pour 0.8 kg - 1.3 kg of leak repair material into the pipe of the leaking equipment from the water inlet, quickly restore the water inlet pipe, and turn on the water inlet. The operation takes only 10 to 15 minutes.
[0030] The water inlet must be opened slowly and not quickly to prevent the leakage repair materials from clogging the pipes or being washed away by the circulating water. After the leaking point of the leaking equipment is successfully repaired, the circulating water valve must not be opened and closed at will to prevent the leakage repair materials from falling off.
[0031] It should be noted that the water inlet pipes and asbestos rubber pipes of the leaking equipment must be easy to disassemble and assemble to facilitate the rapid addition of leak-proof materials. The asbestos rubber pipes must be fireproof and high-temperature resistant.
[0032] Unblocking steps:
[0033] When a leak is found, a compressed air pipeline must be prepared at all times. When the pipeline of the leaking equipment is blocked, connect the compressed air pipeline to the water inlet and outlet of the leaking equipment for quick blowing.
[0034] In the present invention, the calcium carbide furnace is a closed calcium carbide furnace with a capacity of 34.5MVA. The outer diameter of the furnace body is 9900mm, and the furnace cover area equipment includes a furnace cover, a center furnace cover, a water cooling sleeve, a sealing ring, a feed nozzle, an observation door, an explosion-proof hole, a maintenance hole and a pressure detection hole.
[0035] The leak-proof material includes one or a mixture of blue charcoal, coke and electrode paste particles. Specifically, the particle size of the blue charcoal, coke and electrode paste particles is 1-3 mm, and the ratio of blue charcoal, coke and electrode paste particles is 2:2:1.
[0036] When preparing the leak-proof material, firstly select the lignite, coke and electrode paste particles, then air-dry the lignite, coke and electrode paste particles, and then evenly mix the dried lignite, coke and electrode paste particles.
[0037] In the selection of leak repair materials, the use environment of leak repair materials is relatively harsh due to the high temperature, electric and magnetic fields, fast circulating water flow rate and corrosion inhibitors in the calcium carbide furnace cover area. Therefore, the material is required to meet the requirements of high temperature resistance, corrosion resistance, erosion resistance, small difference between material density and circulating cooling water density, insoluble in water and corrosion inhibitors, non-magnetic, and irregular appearance to meet the requirements of leaks of different shapes. Semi-coke, coke and electrode paste particles meet the above requirements.
[0038] In addition, the density of blue carbon is 0.68-0.77g / cm 3 The density of coke is 0.88-1.08g / cm 3 The density of the electrode paste is 1.90-1.96 g / cm 3The density of semi-coke particles is smaller than that of water, so it is easy to repair the upper leak during the repair process; the density of coke particles is similar to that of water, so it can be fully mixed with circulating water and is suitable for repairing hidden leaks; the density of electrode paste particles is larger than that of circulating water, so it is suitable for repairing bottom leaks. However, excessive use of repair materials and excessive particle size can easily clog pipes and equipment, so the particle size and amount of repair materials must be strictly controlled.
[0039] During repair, the sealing material is passed into the pipeline of the leaking equipment and adhered to the leaking point. Since the sealing material is cooled in the circulating water, it is not affected by the high temperature of the furnace surface. The circulating water pressure reaches 0.45MPa, which is much greater than the normal or abnormal furnace pressure. The new composite sealing material at the leaking point is not easy to be washed away. After the repair is completed, it is not affected by the high pressure and high temperature generated by the large collapse of materials. In addition, the sealing material is easy to make and is a common material, which is convenient for material selection and preparation.
[0040] When using welding to repair leaks, it is necessary to remove all circulating water in the equipment, which takes a long time. In addition, the furnace surface temperature is between 400-600℃. When the welding time is long, the temperature of the furnace cover equipment rises quickly. When water is passed through again, the equipment changes greatly between hot and cold, and the stress inside the equipment increases, which will cause the equipment to deform and age faster. At the same time, it is difficult to find cracks when the furnace is stopped for welding, and it is easy for the repair to be incomplete.
Claims
1. A method for repairing leakage of water cooling equipment of calcium carbide furnace, characterized in that: The following steps are involved: Steps for detecting the size and location of the leak: shut down the calcium carbide furnace, check the leak of the calcium carbide furnace, and determine the size and location of the leak; Leak repair steps: When the size of the leak meets the preset size and the location of the leak meets the preset location, turn off the water inlet, remove the water inlet pipe of the leaking equipment, pour the repair material from the water inlet into the pipe of the leaking equipment, reinstall the water inlet pipe, and then turn on the water inlet; The preparation method of the leak-proof material is as follows: selecting blue charcoal, coke and electrode paste particles; drying the blue charcoal, coke and electrode paste particles; uniformly mixing the dried blue charcoal, coke and electrode paste particles; selecting blue charcoal, coke and electrode paste particles with a particle size of 1-3 mm, and uniformly mixing the blue charcoal, coke and electrode paste particles in a ratio of 2:2:1 after drying.
2. A method for repairing leakage of water cooling equipment of calcium carbide furnace according to claim 1, characterized in that: The preset size of the leak point is that the diameter of a single leak point is less than 3 mm, and the preset positions of the leak point are the furnace cover, center furnace cover and water cooling jacket equipment.
3. A method for repairing leakage of water cooling equipment of calcium carbide furnace according to claim 1, characterized in that: After removing the water inlet pipe, connect the asbestos rubber pipe at the water inlet and pour the leak-proof material through the asbestos rubber pipe.
4. A method for repairing leakage of water cooling equipment of calcium carbide furnace according to claim 1, characterized in that: After reinstalling the water inlet pipe, slowly turn on the water inlet.
5. A method for repairing leakage of water cooling equipment of calcium carbide furnace according to claim 1, characterized in that: The method also includes a clearing step: when the pipeline of the leaking equipment is blocked, the compressed air pipeline is connected to the water inlet and outlet of the leaking equipment.