Preparation and application of a polymer material containing strong organic base

By preparing organic polymer materials containing strong organic cations and imidazole anions, the problem of existing catalyst recovery has been solved, and the efficient synthesis of 3-phenyl-2-oxazolidinone under mild conditions has been achieved, which has the advantages of being economical and environmentally friendly.

CN116041602BActive Publication Date: 2024-11-15FUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310017327.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-06
Publication Date
2024-11-15
Estimated Expiration
2043-01-06

AI Technical Summary

Technical Problem

Existing catalysts exhibit high catalytic activity but also high cost, complexity, or difficulty in recovery during the synthesis of 3-phenyl-2-oxazolidinone from CO2 with ethylene oxide and aniline. In particular, ionic liquid catalysts are difficult to separate from the product.

Method used

By preparing organic polymer materials containing strong organic base cations and imidazole anions, and utilizing them to catalyze the synthesis of 3-phenyl-2-oxazolidinone from CO2 with aniline and ethylene oxide at lower temperatures and pressures, the problem of catalyst recovery is solved by using polymerization to bond the strong organic base cations and imidazole anions into the polymer backbone.

Benefits of technology

The synthesis of 3-phenyl-2-oxazolidinone in high yield under mild conditions was achieved, reducing catalyst cost, exhibiting good recoverability and versatility, and significantly improving catalytic activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116041602B_ABST
    Figure CN116041602B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of polymer material synthesis, discloses a preparation and application of a polymer material containing organic strong base, and specifically applies the principle of free polymerization between double bonds of propylene functionalized organic strong base, and prepares an organic polymer material containing organic strong base ions by polymerization reaction of organic strong base ionic liquid and divinylbenzene. The polymer material has good stability, and the synthesis process is simple, the economic cost is low, and it is green and environmentally friendly. The present invention uses the prepared organic strong base polymer material as a catalyst to catalyze the reaction of carbon dioxide and aniline and ethylene oxide to synthesize 3-phenyl-2-oxazolidinone, and shows good catalytic performance under relatively mild reaction conditions and in a relatively short time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer material synthesis, and specifically involves preparing a polymer material containing a strong organic base through a polymerization reaction and applying the polymer material to catalytic conversion of carbon dioxide. Background Art

[0002] With the rapid increase of CO2 emissions due to economic and social development, the current concentration of CO2 in the atmosphere has far exceeded the safe value, inducing a series of environmental problems. Reducing the concentration of CO2 in the atmosphere is one of the urgent problems to be solved. At the same time, CO2, as a cheap and readily available C1 resource, is widely used in the production and synthesis of chemical products such as urea, methanol, carbonates and oxazolidinone. 3-Phenyl-2-oxazolidinone is an important heterocyclic compound. It has received widespread attention because it exhibits multiple pharmacological activities. 3-Phenyl-2-oxazolidinone can be used as a skeleton to synthesize drugs with various uses. For example, the antibiotic drug Zyvox linezolid, the antibacterial drug Sivextro, and the antidepressant Humoryl. In addition, oxazolidinone has good photochemical and photophysical activity and can be used in semiconductor devices such as electrophoretic photoreceptors and nonlinear optical materials. The traditional synthesis method of 3-aryl-2-oxazolidinone is through the reaction of phosgene with 2-alkylamine and the reaction of isocyanate with epoxide. Phosgene and isocyanate are considered to be non-green toxic raw materials and have been gradually eliminated. In recent years, a new method for directly synthesizing 3-phenyl-2-oxazolidinone from carbon dioxide, aniline, and ethylene oxide has been reported. This method uses cheap and readily available raw materials, converts carbon dioxide into high-value-added 3-phenyl-2-oxazolidinone, takes into account both environmental and economic benefits, and has broad development prospects.

[0003] At present, the method of directly synthesizing 3-phenyl-2-oxazolidinone from CO2, ethylene oxide and aniline contains three reactions. The catalyst must be able to catalyze the CO2 cycloaddition reaction, activate aniline and the intermediate product N-phenylethanolamine, and quickly convert the intermediate product into the final product 3-phenyl-2-oxazolidinone to avoid side reactions that lead to a decrease in product yield. The catalysts currently studied are mainly concentrated on composite catalysts, base catalysts, and ionic liquid catalysts. Composite catalysts include DMEDA / IL–NH2-MIL-101, PVA-DFNT / Ni, etc. These catalysts have high catalytic activity, low dosage, convenient recycling and good repeatability, but have the disadvantages of high catalyst cost and complex synthesis. The main base catalysts are K3PO4, TBAI, etc. This type of catalyst has high catalytic activity and low cost. However, it has the disadvantages of large dosage and the need for solvents or co-catalysts. Ionic liquids are a type of molten salt composed of organic cations and organic anions or inorganic anions. The anions and cations interact with each other through electrostatics and hydrogen bonds. They are liquid at room temperature or near room temperature and have low vapor pressure, good solubility, high stability, adjustable acidity, etc. They have good solubility and affinity for CO2 and good catalytic activity in CO2 fixation reactions. However, they have the disadvantages of high viscosity and difficulty in recycling. The yield of the reaction product catalyzed by ionic liquids BmimBr+BmimOAc and HDBUBr+DBU is over 93%. The catalyst cost is low and the catalytic activity is good, but there is a disadvantage that the catalyst is difficult to recover from the product.

[0004] The present invention designs an organic polymer material containing organic base cations and imidazolium anions, and realizes a high yield of 3-phenyl-2-oxazolidinone under the conditions of lower reaction temperature and pressure and shorter time. The polyionic liquid organic polymer material prepared by the present invention contains organic base cations and imidazolium anions, and has good adsorption to CO2. The organic base cations can cooperate with the anions to carry out electrophilic attack and nucleophilic attack, activate ethylene oxide to open its ring, and the open-ring ethylene oxide and carbon dioxide undergo cycloaddition to generate ethylene carbonate. The imidazolium anion can capture hydrogen atoms on the amino group of aniline, activate aniline to react with the open-ring ethylene oxide to generate N-phenylethanolamine; the imidazolium anion can also activate N-phenylethanolamine by capturing hydrogen atoms on hydroxyl and imino groups, and generate 3-phenyl-2-oxazolidinone with ethylene carbonate. Summary of the invention

[0005] The main purpose of the present invention is to prepare an organic polymer material containing organic strong base cations and imidazolium anions through polymerization reaction and its application in rapidly catalyzing CO2, aniline and ethylene oxide to synthesize 3-phenyl-2-oxazolidinone under relatively mild conditions.

[0006] In order to achieve the above-mentioned purpose of the invention, the present invention adopts the following technical solutions:

[0007] Preparation of organic strong base polymer material: First, simply functionalize the organic strong base propylene group to prepare ionic liquid 1, and use ion exchange resin to replace the anion of ionic liquid 1 to prepare ionic liquid 2. Ionic liquid 2 reacts with imidazole to prepare ionic liquid 3. Ionic liquid 3 and divinylbenzene are used to undergo polymerization under the action of a chain initiator, and the organic base cation and anion are bonded to the polymer skeleton through covalent bonds. Specific synthesis steps:

[0008] (1) dissolving an organic strong base in an organic solvent to prepare solution A; weighing halogen-containing propylene in a certain proportion and dissolving it in an organic solvent to prepare solution B; then dropping solution A into solution B, stirring at high temperature for a period of time, and removing the solvent to obtain a brown viscous liquid, which is the propylene-functionalized organic strong base ionic liquid 1;

[0009] (2) dissolving ionic liquid 1 in an organic solvent to prepare solution C, placing an ion exchange resin in a chromatography column as a stationary phase, and using solution C as a mobile phase to perform anion exchange, exchanging anions in ionic liquid 1 with hydroxyl anions, and removing the solvent to obtain a light yellow viscous liquid, which is the propylene-functionalized organic strong base ionic liquid 2;

[0010] (3) Dissolving ionic liquid 2 in an organic solvent to prepare solution D; weighing a compound containing an imidazole group in a certain proportion and dissolving it in an organic solvent to prepare solution E; adding solution D dropwise into solution E, stirring at high temperature for a period of time, and removing the solvent to obtain a light brown viscous liquid, which is the propylene functionalized organic strong base ionic liquid 3;

[0011] (4) Dissolve the ionic liquid 3 and divinylbenzene in an organic solvent respectively to obtain solution F and solution G; then add solution F dropwise into solution G, and then add a chain initiator, stir at room temperature for 30 min, and after the added substances are fully dissolved, heat in an oil bath under a nitrogen atmosphere for a period of time, wash and dry to obtain the polymer material containing a strong organic base.

[0012] The organic solvent in the above steps (1), (2), (3), and (4) is one of methanol, ethanol, acetonitrile, and ethyl acetate.

[0013] The organic strong base in the above step (1) is one of tetramethylguanidine (TMG), 1,8-diazabicycloundec-7-ene (DBU) and 1,5-diazabicyclo[4.3.0]-5-nonene (DBN);

[0014] The halogen-containing propene in the above step (1) is one of 3-bromopropene and 3-chloropropene;

[0015] The molar ratio of the halogen-containing propene to the organic strong base in the above step (1) is between 1.0:1.0 and 1.0:6.0;

[0016] In the above step (1), the high temperature stirring temperature is 70-120°C and the time is 6-12h.

[0017] The compound containing an imidazole group in the above step (3) is one of imidazole, 1-methylimidazole and 2-methylimidazole;

[0018] In the above step (3), the molar ratio of the compound containing an imidazole group to the ionic liquid 2 is between 1.0:1.0 and 1.0:6.0;

[0019] The chain initiator in the above step (4) is azobisisobutyronitrile (AIBN).

[0020] In the above step (4), the heating reaction temperature is 70-120°C and the time is 6-12h;

[0021] In the above step (4), the molar ratio of the ionic liquid 3 to divinylbenzene is between 0.2:1.0 and 2.0:1.0.

[0022] The present invention applies an organic polymer material containing organic strong base cations and imidazole anions to CO2, aniline and ethylene oxide to synthesize 3-phenyl-2-oxazolidinone. The specific operation is as follows: aniline, ethylene oxide and the organic strong base polymer material are added into a 100 ml high-pressure reactor, and the CO2 pressure is 1-3 MPa, the reaction temperature is 100-140°C, and the reaction is stirred for 1-9 hours to prepare 3-phenyl-2-oxazolidinone.

[0023] The beneficial effects of the present invention are:

[0024] The present invention utilizes the structural characteristics of the double bonds on the propylene functionalized organic strong base, with divinylbenzene as the skeleton, under the action of a chain initiator, the double bonds on the propylene functionalized organic strong base can be freely polymerized with the divinylbenzene skeleton, and the material contains organic strong base cations and imidazole anions, which can catalyze three reactions in the system. The composite material prepared by the method solves the problem that ionic liquids are difficult to recover from the reaction system. Compared with other heterogeneous catalysts, it has the advantages of low economic cost and green material environment. The organic composite material prepared by the present invention is used as a catalyst, applied to carbon dioxide and aniline, ethylene oxide directly synthesizes 3-phenyl-2-oxazolidinone, and a higher 3-phenyl-2-oxazolidinone yield can be achieved in a relatively short time. In addition, the method has certain universality, and a variety of functionalized ionic liquids and divinylbenzene can achieve effective synthesis of composite materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1The structural formula of P-AD-1 / 1 and its preparation process;

[0026] Figure 2 XRD spectra of P-AD-0 / 1 and P-AD-1 / 1;

[0027] Figure 3 The infrared spectra of P-AD-0 / 1, [AIDBU]Im and P-AD-1 / 1;

[0028] Figure 4 is the scanning electron microscopy image of P-AD-0 / 1 and P-AD-1 / 1;

[0029] Figure 5 The catalytic activities of P-AD-0 / 1, P-AD-1 / 0, P-AD-1 / 2, and P-AD-1 / 1;

[0030] Figure 6 This is the recycling performance of P-AD-1 / 1 catalyst. Specific implementation methods

[0031] The present invention is further described by the following specific examples, but the protection scope of the present invention is not limited to the following examples.

[0032] Example 1

[0033] (1) Synthesis of allyl bromide functionalized DBU ([AIDBU]Br)

[0034] Weigh 10 mmol of 3-bromoallyl and dissolve it in 10 mL of acetonitrile to prepare solution A. Weigh 10.5 mmol of DBU and dissolve it in 10 mL of acetonitrile to prepare solution B. Add solution A dropwise into solution B. Under nitrogen protection, stir magnetically at 70 °C for 24 h. Remove the solvent, wash three times with n-heptane and dry to obtain a brown viscous liquid, which is bromoallyl functionalized DBU ([AIDBU]Br).

[0035] (2) Synthesis of allyl bromide functionalized DBU ([AIDBU]Im)

[0036] Weigh 10 mmol of [AIDBU]Br and dissolve it in 10 ml of methanol to prepare solution C. Use pretreated anion exchange resin as the stationary phase and solution C as the mobile phase. After exchanging anions, remove the solvent and dry to obtain a light yellow liquid, which is [AIDBU]OH; weigh 10 mmol of [AIDBU]OH and dissolve it in 10 ml of methanol to prepare solution D, weigh 10.5 mmol of imidazole and dissolve it in 10 ml of methanol to prepare solution E, add solution D dropwise to solution E, and stir magnetically at 60 °C for 24 h under nitrogen protection. Remove the solvent and dry to obtain a brown liquid, which is [AIDBU]Im.

[0037] (3) Synthesis of organic strong base polymer P-AD-1 / 1

[0038] Weigh 10 mol of [AIDBU]Im and dissolve it in 10 ml of ethanol to prepare solution F. Weigh 10 mol of divinylbenzene and dissolve it in 10 ml of ethanol to prepare solution G. Add solution F dropwise into solution G. Transfer the mixed solution to a three-necked flask and add 0.1 mmol of AIBN. Stir at room temperature for 30 min. After the added substances are fully dissolved, stir magnetically at 80 °C for 24 h under a nitrogen atmosphere. Collect the white precipitate, wash and dry it with ethanol and ethyl acetate to obtain the organic strong base polymer material P-AD-1 / 1. (1 / 1 represents the mmol of [AIDBU]Im and divinylbenzene added respectively)

[0039] (4) Synthetic organic polymer P-AD-0 / 1

[0040] Weigh 10 mol of divinylbenzene and dissolve it in 10 ml of ethanol and transfer it to a three-necked flask. Then add 0.05 mmol AIBN and stir it at room temperature for 30 min. After the added substance is fully dissolved, stir it magnetically at 80 °C for 24 h under a nitrogen atmosphere. Collect the white precipitate, wash it with ethanol and ethyl acetate, and dry it to obtain the polymer material P-AD-0 / 1 that does not contain organic strong base.

[0041] (2) Synthesis of P-AD-1 / 0

[0042] Weigh 10 mol of [AIDBU]Im and dissolve it in 10 mL of ethanol. Transfer it to a three-necked flask, then add 0.05 mmol AIBN and stir it at room temperature for 30 min. After the added substance is fully dissolved, stir it magnetically at 80 °C for 24 h under a nitrogen atmosphere to obtain a brown-yellow liquid. It can be seen that [AIDBU]Im cannot be polymerized alone without the addition of divinylbenzene. The product obtained is [AIDBU]Im monomer. After washing and drying with ethanol and ethyl acetate, the material P-AD-1 / 0 without the polymer skeleton DVB can be obtained.

[0043] Figure 1 This is the molecular structure of the organic strong base polymer material P-AD-1 / 1 prepared in this embodiment.

[0044] Figure 2 : is the XRD spectrum of the organic strong base polymer material P-AD-1 / 1 prepared in this example. It can be observed from the XRD spectrum that P-AD-1 / 1 has a broad peak centered at about 2θ=18°, which indicates that P-AD-1 / 1 is amorphous, which is caused by the disordered stacking of the polymer.

[0045] Figure 3 The infrared spectra of the pure ionic liquid [AIDBU]Im, P-AD-0 / 1 and the organic strong base polymer material P-AD-1 / 1 prepared in this embodiment are shown in FIG. As can be seen from the figure, the spectrum of P-AD-1 / 1 is almost the same as that of P-AD-0 / 1, and no characteristic peak of [AIDBU]Im is observed. It is speculated that the amount of [AIDBU]Im polymerized on DVB is relatively small, and the characteristic peak is covered.

[0046] Figure 4 The following are scanning electron microscope images of the organic polymer materials P-AD-0 / 1 and P-AD-1 / 1 prepared in this example. It can be seen from the figure that the organic polymer P-AD-0 / 1 without [AIDBU]Im loading is in the shape of a regular sphere with a smooth surface, while the organic strong base polymer P-AD-1 / 1 loaded with [AIDBU]Im has obviously become smaller and irregular in shape, indicating that [AIDBU]Im has been successfully bonded to the polymer skeleton. Figure 3 It is speculated that [AIDBU]Im has a large steric hindrance, is difficult to polymerize onto the backbone, and will reduce the degree of polymerization of the polymer.

[0047] Figure 5 The organic base polymer materials P-AD-0 / 1, P-AD-1 / 0, P-AD-1 / 2, and P-AD-1 / 1 prepared in this embodiment were compared in terms of the yield of 3-phenyl-2-oxazolidinone under the conditions of reaction temperature 110 °C, 2.5 MPa CO2, and reaction time 1h. The results show that under the same reaction conditions, when P-AD-1 / 0, i.e., [AIDBU]Im monomer, is used as the catalyst, the product yield is 50%; however, the polymer materials P-AD-1 / 2, P-AD-1 / 1, and P-AD-0 / 1 have DMC yields of 56%, 66%, and 28%, respectively. This indicates that after [AIDBU]Im is bonded to the polymer backbone through polymerization reaction, it can increase the active sites of organic base groups and imidazole groups, thereby increasing the probability of contact between the catalyst and CO2 and further promoting the reaction; for P-AD-1 / 0, for catalysts of the same mass, the imidazole active sites of P-AD-1 / 1 are limited, which may reduce the occurrence of side reactions, resulting in a higher product yield than P-AD-1 / 0, and there is no imidazole group on P-AD-0 / 1, so this is also the reason for the low catalytic activity of P-AD-0 / 1; in addition, the yield of 3-phenyl-2-oxazolidinone when the molar ratio of [AIDBU]Im and divinylbenzene is 1:1 is higher than that when the molar ratio is 1:2, which may be because there are more active sites of the imidazole group.

[0048] Table 1 is an elemental analysis table of the polymer material P-AD-0 / 1 and the organic strong base polymer material P-AD-1 / 1 prepared in this example.

[0049] Table 1 Elemental analysis of polymer material P-DVB and organic strong base polymer material P-AD-1 / 1

[0050]

[0051] The results showed that [AlDBU]IM was successfully polymerized on the P-DVB backbone.

[0052] Application Example 1

[0053] Weigh 4.4 g of ethylene oxide, 0.744 g of aniline, and 0.15 g of catalyst P-AD-1 / 1, add them into a high-pressure reactor, fill with 1.0 MPa CO2, and react with stirring at 110 ℃ for 1 hour. After the reaction, take 15 ml of chloroform to dissolve the product, filter out the catalyst, and wash it three times with 15 ml of deionized water. Take the organic phase for gas chromatography analysis to calculate the yield of 3-phenyl-2-oxazolidinone. Through single factor experiment, the yield of 3-phenyl-2-oxazolidinone gradually increased with the increase of catalyst dosage until the catalyst dosage reached its equilibrium point of 0.15 g; as the reaction temperature first increased and then decreased, at 110 ℃, the yield of 3-phenyl-2-oxazolidinone reached its peak value, because the reaction was an exothermic reaction, and the temperature was too high, which was not conducive to the forward reaction; as the CO2 pressure increased, the yield of 3-phenyl-2-oxazolidinone showed an upward trend, reaching a peak value at a pressure of 2.5Mpa; the yield of 3-phenyl-2-oxazolidinone remained unchanged as the reaction time increased, and the reaction reached equilibrium after 1h. Therefore, under the optimal reaction conditions (110 ℃, 2.5 MPa, 1 h), the yield of 3-phenyl-2-oxazolidinone was 66%.

[0054] Table 2 is a comparison of the catalytic performance of P-AD-1 / 1 prepared in the example with other catalysts. As shown in Table 2, compared with HDBUBr+DBU and BmimBr+BmimOAc catalysts, P-AD-1 / 1 has a 3-phenyl-2-oxazolidinone yield of 66% under relatively mild conditions. Compared with the above two liquid catalysts, P-AD-1 / 1 can achieve simple catalyst recycling; under the same conditions, compared with P-AD-0 / 1 without organic strong base groups, the catalytic activity of the prepared organic polymer material P-AD-1 / 1 is greatly improved.

[0055] Table 2 Comparison of catalytic performance of P-AD-1 / 1 and other types of catalysts

[0056]

[0057] Figure 6The cyclic performance of the P-AD-1 / 1-catalyst prepared in the embodiment is shown. After five cycles of use, the conversion rate of aniline is still maintained at more than 99%, and the yield of 3-phenyl-2-oxazolidinone is maintained at 66% in the first four cycles and decreased to 64% in the fifth cycle. Within the experimental error range, the catalyst performance remains basically unchanged, and the catalyst shows excellent cyclic performance.

[0058] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. An application of a polymer material containing an organic strong base, characterized in that: The organic base-containing polymer material is used as a catalyst in the reaction of CO2 with aniline and ethylene oxide to synthesize 3-phenyl-2-oxazolidinone. The specific operation is as follows: aniline, ethylene oxide and the organic base-containing polymer material are added into a 100 ml high-pressure reactor, and the CO2 pressure is 1-3 MPa, the reaction temperature is 100-140 °C, and the reaction is stirred for 1-9 hours to prepare 3-phenyl-2-oxazolidinone. The method for preparing the organic strong base polymer material comprises the following steps: (1) dissolving an organic strong base in an organic solvent to prepare solution A; weighing halogen-containing propylene in a certain proportion and dissolving it in an organic solvent to prepare solution B; then dropping solution A into solution B, stirring at high temperature for a period of time, and removing the solvent to obtain a brown viscous liquid, which is the propylene-functionalized organic strong base ionic liquid 1; (2) dissolving ionic liquid 1 in an organic solvent to prepare solution C, placing an ion exchange resin in a chromatography column as a stationary phase, and using solution C as a mobile phase to perform anion exchange, exchanging anions in ionic liquid 1 with hydroxyl anions, and removing the solvent to obtain a light yellow viscous liquid, which is the propylene-functionalized organic strong base ionic liquid 2; (3) Dissolving ionic liquid 2 in an organic solvent to prepare solution D; weighing a compound containing an imidazole group in a certain proportion and dissolving it in an organic solvent to prepare solution E; adding solution D dropwise into solution E, stirring at high temperature for a period of time, and removing the solvent to obtain a light brown viscous liquid, which is the propylene functionalized organic strong base ionic liquid 3; (4) Dissolve the ionic liquid 3 and divinylbenzene in an organic solvent respectively to obtain solution F and solution G; then add solution F dropwise into solution G, and then add a chain initiator, stir at room temperature for 30 min, and after the added substances are fully dissolved, heat in an oil bath under a nitrogen atmosphere for a period of time, wash and dry to obtain the polymer material containing a strong organic base.

2. The use according to claim 1, characterized in that: The organic solvent in steps (1), (2), (3), and (4) is one of methanol, ethanol, acetonitrile, and ethyl acetate.

3. The use according to claim 1, characterized in that: The organic strong base in step (1) is one of tetramethylguanidine, 1,8-diazabicycloundec-7-ene and 1,5-diazabicyclo[4.3.0]-5-nonene; the halogen-containing propene is one of 3-bromopropene and 3-chloropropene; and the molar ratio of the halogen-containing propene to the organic strong base is between 1.0:1.0 and 1.0:6.

0.

4. The use according to claim 1, characterized in that In step (1), the high temperature stirring temperature is 70-120°C and the time is 12-24h.

5. The use according to claim 1, characterized in that : The compound containing imidazole group in step (3) is one of imidazole, 1-methylimidazole and 2-methylimidazole; the molar ratio of ionic liquid 2 to the compound containing imidazole group is between 1.0:1.0 and 1.0:6.

0.

6. The use according to claim 1, characterized in that: The chain initiator was azobisisobutyronitrile.

7. The use according to claim 1, characterized in that : In step (4), the heating reaction temperature is 70-120°C and the time is 12-24h.

8. The use according to claim 1, characterized in that : In step (4), the molar ratio of ionic liquid 3 to divinylbenzene is between 0.2:1.0 and 2.0:1.0.