Preparation method of scale inhibitor for inhibiting formation of calcium carbonate scale in geothermal wellbore during high-temperature geothermal water utilization
By preparing AA-HEMA-SAS-CA-MSG copolymer as scale inhibitor during the use of high-temperature geothermal water, the problem of calcium carbonate scale formation in geothermal wellbore is solved, and efficient scale inhibition effect is achieved, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202310121504.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-16
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-02-16
AI Technical Summary
The formation of calcium carbonate scale caused by geothermal fluid under temperature and pressure changes in geothermal wellbores leads to increased flow resistance, increased equipment energy consumption, and may block the wellbore, reducing the yield and utilization rate.
Develop a scale inhibitor used to inhibit the formation of calcium carbonate scale in geothermal wellbores during the use of high-temperature geothermal water. By reacting acrylic acid, hydroxyethyl methacrylate, sodium allylsulfonate, citric acid and gluten in a three-neck flask Five monomers including sodium amide were prepared, and the pH value was adjusted by potassium hydroxide, and anhydrous methanol precipitation and filtration under reduced pressure were obtained to obtain purified scale-resistance agent.
The scale inhibitor maintains a scale resistance of more than 94% under the conditions of 150°C to 200°C, effectively solving the problem of calcium carbonate scale adhesion on the surface of the geothermal wellbore, improving the circulation efficiency of geothermal fluids, and low cost and low environmental pollution. Suitable for industrial applications.
Smart Images

Figure CN116041608B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to geothermal wellbore scale prevention and removal, and in particular to a scale inhibitor used in the process of utilizing high-temperature geothermal water to inhibit the formation of calcium carbonate scale attached to the wall of a geothermal wellbore. Background Art
[0002] The overall distribution of geothermal energy in my country shows the characteristics of “high in the east and low in the west, high in the south and low in the north”. The overall thermal background in the continental region is not high, with an average geothermal heat flux density of 63MW / m 2 (Wang Jiyang. Geothermal Science and Its Applications [M]. Beijing: Science Press, 2015). In the process of geothermal energy extraction, the original chemical balance of geothermal fluid will be destroyed after the pressure and temperature of geothermal fluid in the geothermal wellbore change, so scaling is easy to occur in the geothermal wellbore. The scaling of geothermal fluid on the wellbore will sharply increase the flow resistance of geothermal fluid, and at the same time increase the energy consumption of geothermal equipment. In severe cases, it may even block the geothermal wellbore, causing production to stagnate, thereby reducing the recovery rate and utilization rate of geothermal wells (Topcu, G, Koc, GA., Baba, A, et al. The injection of CO2 to hypersaline geothermal brine: A case study for Tuzla region. Geothermics (Geothermics), 2019, 80: 86-91). However, cleaning the dirt on the wellbore wall will increase the cost of operation and maintenance (Béatrice AL, Ronan LH, Justine M, et al. Scaling in a Geothermal Heat Exchanger at Soultz-Sous-Forêts (Upper Rhine Graben, France): A XRD and SEM-EDS Characterization of Sulfide Precipitates (Soultz Sous Foréts (Upper Rhine Graben, France) geothermal heat exchanger scaling: XRD and SEM-EDS characterization of sulfide precipitation. Geosciences (Earth Science), 2021, 11 (7): 271), and will also cause many production safety problems ( G, Weiser L, et al. Study of calcite scaling and corrosion processes in geothermal systems. Geothermics, 2000, 29 (1): 105-119). In the development of geothermal energy in Sichuan, Tibet and North China, scaling phenomena have been found to varying degrees (Wang Yanxin, Liu Shiliang, Bian Qingyu, et al. Scaling analysis and anti-scaling measures of geothermal wells in Ganzi. Progress in New Energy, 2015, 3 (3): 202-206). The most common scaling in geothermal fluids is calcium carbonate scaling. Therefore, it is necessary to develop a scale inhibitor with better performance to solve the scaling problem caused by changes in temperature and pressure during the ascent of geothermal fluids in the wellbore. Although the scaling problem of geothermal fluids is very complex and is a dynamic process, from the fundamental reason, the geothermal fluids have become supersaturated solutions of CO2 after billions of years of geological movement in the strata, so there is a large amount of HCO3 in the geothermal fluids. - When the geothermal fluid rises along the geothermal wellbore, as the pressure of the geothermal fluid in the geothermal well continues to decrease, when the partial pressure of the geothermal water in its liquid phase is lower than the saturated vapor pressure corresponding to the temperature during the rise, an obvious flash phenomenon will occur. After the geothermal fluid flashes, the geothermal fluid will change from the original single-phase flow to gas-liquid two-phase flow, and at this time the water vapor in the gas phase will increase rapidly, diluting the CO2 in the gas phase; at the same time, the intrusion of other non-condensable gases (such as CH4, N2 and H2S gases) and the corrosion of the geothermal wellbore will also cause a large reduction in the original CO2 gas in the gas phase, so that the CO2 partial pressure in the gas phase will decrease rapidly; at the same time, the CO2 gas dissolved in the geothermal fluid will be released into the gas phase in large quantities (causing the reaction equation (1) to proceed to the right), which increases the pH value in the geothermal fluid and dilutes the supersaturated HCO3 in the geothermal fluid. - The dissociated H + Neutralization (reaction equation (2) proceeds to the right), eventually leading to the generation of a large amount of CO3 in the geothermal fluid 2- , and the large amount of Ca originally present in the geothermal fluid 2+ The combination causes the precipitation of calcium carbonate and scaling (reaction equation (3) proceeds to the right), thereby adhering to the inner wall of the geothermal wellbore.
[0003]
[0004]
[0005]
[0006] In summary, there are two main factors that affect geothermal fluid scaling: (1) the supersaturated state of geothermal fluids and the very complex chemical composition; (2) the changes in temperature and pressure during the ascent of geothermal fluids, which causes changes in the flow state of the fluid, thereby affecting the dissolution-precipitation balance of calcium carbonate minerals.
[0007] Researchers from many domestic and foreign enterprises and research institutes have conducted a lot of theoretical and experimental research on the calcium carbonate scaling of geothermal fluids. In 1978, Epstein proposed the scaling layer deposition theory at the 6th International Heat Transfer Conference, and divided the formed scale into six types according to the physical / chemical process, namely, crystal scale, corrosion scale, chemical reaction scale, biological scale, coagulation scale, and particle scale. Later, mixed scale was added. Mixed scale is usually the result of the simultaneous action of the above-mentioned scaling mechanisms (Epstein N. Thinking about Heat Transfer Fouling: A 5×5 Matrix, Heat Transfer Engineering, 1983, 4: 1, 43-56). In 1983, Epstein divided the scale formation process into five stages based on the five stages of initiation, transport, attachment, erosion and aging. This division has taken human understanding of scale a step further. Yang Shanrang proposed that fouling refers to a layer of soft mud or solid material accumulated on the surface of equipment in contact with fluid, and its existence is generally a mixture. Therefore, the fouling of geothermal fluid is also an irreversible process from the clean state of the surface of geothermal equipment to being covered with calcium carbonate scale (Yang Shanrang. Fouling and Countermeasures of Heat Exchange Equipment [M]. Beijing: Science Press, 2004).
[0008] Regarding the removal of geothermal fluid scale, relevant researchers have also done a lot of research and attempts. For example, Gallup et al. proposed to adjust the pH value of geothermal fluid to less than 4.5 to achieve the purpose of geothermal fluid scale prevention (Gallup DL. Brine pH modification scale control technology. A review). Transactions-Geothermal Resources Council, 2011, 35 (1): 609-614.). Tonaszewska et al. used composite ultrafiltration-reverse osmosis membrane filtration to remove elements such as boron, iron and arsenic in geothermal fluid. The geothermal fluid after filtration was tested and found to be able to be discharged into surface waters (Tomaszewska B, Bodzek M. Desalination of geothermal water using a hybrid UF-RO process. Desalination, 2013, 319: 99-106). There are three main methods: physical removal, mechanical removal and chemical removal (Bott TR. Fouling of Heat Exchangers. Experimental Thermal and Fluid Science, 1997, 14(4): 315.).
[0009] Mechanical cleaning methods may leave rough pits on the surface of the equipment, which has a serious impact on the safety of the equipment and will also accelerate the accumulation of dirt during the subsequent operation of the equipment. Physical descaling methods cannot remove scale relatively evenly, especially for the complex interior of the equipment, physical descaling cannot completely clean all the dead corners. It is not easy to control the amount of acid used when using chemical acid treatment. When the amount of chemical acid is too much, it is easy to corrode the geothermal well and the equipment on the well, causing a certain degree of loss. In summary, adding chemical scale inhibitors to geothermal fluids to inhibit wellbore scaling is an effective method (Dan L, Dong W, Li F, et al. Comparative performance of polyepoxysuccinic acid and polyaspartic acid on scaling inhibition by static and rapid controlled precipitation methods. Desalination, 2012, 304: 1-10.). Moreover, when injecting scale inhibitors, most chemical scale inhibitors also have a certain degree of corrosion inhibition, so as to alleviate the corrosion of chemical scale inhibitors to geothermal systems. The calcium carbonate scale produced by geothermal fluids mainly has three crystal forms, namely calcite, aragonite and vaterite. The calcium carbonate scale of geothermal fluids in the wellbore is generally calcite crystals, because the thermal stability of calcite is the best among the three crystal forms, and the thermodynamic stability of vaterite is the lowest among the three crystal forms. At the same time, vaterite is also the initial phase of calcium carbonate when it is supersaturated. Without adding scale inhibitors, there is a supersaturated calcium carbonate solution in the geothermal fluid. When the temperature and pressure change, the supersaturated calcium carbonate solution will precipitate, thereby precipitating vaterite crystals. Due to the thermodynamic instability of vaterite, vaterite crystals can be easily converted into aragonite and calcite. Because calcite crystals are sharp rhombohedral, when scale inhibitors are added, the calcium carbonate crystals lose their original sharp edges, and the crystal shape changes from rhombohedral to scaly. After adding the scale inhibitor, the vaterite crystals cannot adhere to each other, and the scale inhibitor also turns the hard scale into soft scale, which can be easily washed off. The scale inhibitor mainly adsorbs on the active sites on the surface of the crystal, thereby hindering the nucleation and continued growth of the crystal and changing the structure of the crystal. However, the general scale inhibitor is easily deactivated at high temperature, which reduces the scale inhibition rate. Summary of the invention
[0010] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a scale inhibitor that has high descaling efficiency and is resistant to high temperatures and that can inhibit the formation of calcium carbonate scale in geothermal wellbores during the utilization of high-temperature geothermal water.
[0011] The method for preparing a scale inhibitor for inhibiting the formation of calcium carbonate scale in a geothermal wellbore during the utilization of high-temperature geothermal water of the present invention comprises the following steps:
[0012] The first step is to prepare a three-necked flask, wherein a thermometer is placed at the first neck to detect the temperature change in the flask in real time, a separatory funnel is placed at the second neck to add an initiator, and a reflux condenser is placed at the third neck to reflux and condense organic matter; five monomers, namely acrylic acid, hydroxyethyl methacrylate, sodium allyl sulfonate, citric acid and sodium glutamate, are placed in the three-necked flask, wherein the mass ratio of acrylic acid, hydroxyethyl methacrylate, sodium allyl sulfonate, citric acid and sodium glutamate is (32-60):(4-7):(4-7):(2-4):(3-7);
[0013] In the second step, tert-butanol having a mass ratio of 10% to the total mass of the five monomers is placed in the three-necked flask in the first step, and then deionized water is added to completely dissolve the tert-butanol in the deionized water. The mass fraction of the tert-butanol is 99%, which serves as a molecular weight regulator for the reaction.
[0014] The third step is to place the three-necked flask in a magnetic stirring heater that has been preheated to a temperature between 30°C and 80°C for water bath heating, and after adjusting the temperature of the magnetic stirring heater to 80°C, perform constant temperature heating;
[0015] The fourth step is to pour an ammonium persulfate initiator solution with a mass percentage concentration of 7.27% into a separatory funnel, wherein the mass ratio of the ammonium persulfate in the ammonium persulfate initiator solution to the total mass of the five monomers is 1:10; then adjust the knob of the separatory funnel to drip the ammonium persulfate solution into the reaction solution at a dripping rate of one drop every three to five seconds; after constant temperature heating for three hours, take out the three-necked flask and cool it to between 25°C and 30°C. The obtained copolymer is the scale inhibitor AA-HEMA-SAS-CA-MSG for inhibiting the formation of calcium carbonate scale in geothermal wells during the utilization of high-temperature geothermal water; potassium hydroxide solution is added to the generated copolymer to adjust the pH value of the copolymer solution to 5.0, and the copolymer is precipitated with anhydrous methanol, and the copolymer is dried after vacuum filtration by a suction pump to obtain a purified scale inhibitor.
[0016] The technical effects of the present invention compared with the prior art are:
[0017] (1) The problem of calcium carbonate scale adhesion on geothermal wellbore can be effectively solved by adding a small amount of anti-fouling agent.
[0018] (2) In the scale inhibitor formula, the amount of citric acid and sodium glutamate used is relatively small, the main component is acrylic acid, and the cost is low.
[0019] (3) Low environmental pollution. In the scale inhibitor formula, the five monomers of the scale inhibitor do not contain phosphorus elements and will not cause water pollution after use. Moreover, the five monomers required are easy to obtain and do not require special configuration.
[0020] (4) High temperature resistance: the synthetic scale inhibitor can maintain a scale inhibition rate of more than 94% at high temperatures; it is simple and easy to use, and suitable for industrial applications.
[0021] (5) The problem of calcium carbonate scale adhesion on the surface of geothermal wellbore is solved, and the circulation efficiency of geothermal fluid in the geothermal wellbore is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The synthesis and preparation of the scale inhibitor added in Example 1 for preventing the adhesion of calcium carbonate scale on the surface of the geothermal wellbore during the utilization of geothermal water, as well as the scale inhibition mechanism;
[0023] Figure 2 The scale inhibition rate of the scale inhibitor added to Example 2 for preventing calcium carbonate scale from adhering to the surface of the geothermal wellbore during the utilization of geothermal water and other different scale inhibitors varies with temperature. DETAILED DESCRIPTION
[0024] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the protection scope of the present invention.
[0025] The method of the invention uses a high-temperature and high-pressure reactor to verify the actual scale inhibition rate of the studied scale inhibitor at high temperature, uses a potentiometric titration method to determine the scale inhibition rates of several studied scale inhibitors, and screens out scale inhibitors that meet the requirements.
[0026] The scale inhibition mechanism of the scale inhibitor of the present invention is mainly that the newly synthesized scale inhibitor AA-HEMA-SAS-CA-MSG can chelate with calcium ions in geothermal fluid, thereby inhibiting the formation of calcium carbonate scale in the geothermal fluid.
[0027] like Figure 1 The method for preparing a scale inhibitor for inhibiting the formation of calcium carbonate scale in a geothermal wellbore during the utilization of high-temperature geothermal water of the present invention comprises the following steps:
[0028] The first step is to prepare a three-necked flask, wherein a thermometer is placed at the first neck to detect the temperature change in the flask in real time, a separatory funnel is placed at the second neck to add an initiator, and a reflux condenser is placed at the third neck to reflux and condense organic matter; five monomers, namely acrylic acid (AA), hydroxyethyl methacrylate (HEMA), sodium allyl sulfonate (SAS), citric acid (CA) and sodium glutamate (MSG), are placed in the three-necked flask, wherein the mass ratio of acrylic acid, hydroxyethyl methacrylate, sodium allyl sulfonate, citric acid and sodium glutamate is (32-60):(4-7):(4-7):(2-4):(3-7);
[0029] In the second step, tert-butanol in a mass ratio of 10% to the total mass of the five monomers is placed in the three-necked flask in the first step, and then deionized water is added to make the tert-butanol completely dissolved in the deionized water. The mass fraction (purity) of the tert-butanol is 99%, which serves as a molecular weight regulator for the reaction;
[0030] The third step is to place the three-necked flask in a magnetic stirring heater that has been preheated to a temperature between 30°C and 80°C for water bath heating, and after adjusting the temperature of the magnetic stirring heater to 80°C, perform constant temperature heating;
[0031] The fourth step is to pour the ammonium persulfate initiator solution with a mass percentage concentration of 7.27% into the separatory funnel, wherein the mass ratio of the ammonium persulfate in the ammonium persulfate initiator solution to the total mass of the five monomers is 1:10; then adjust the separatory funnel knob to drip the ammonium persulfate solution into the reaction solution at a drip rate of one drop every three to five seconds to ensure the stable and sufficient reaction. After three hours of constant temperature heating, the three-necked flask is taken out and cooled to between 25°C and 30°C. The obtained copolymer is the scale inhibitor AA-HEMA-SAS-CA-MSG (i.e., scale inhibitor acrylic acid-hydroxyethyl methacrylate-sodium allyl sulfonate-citric acid-sodium glutamate) required in the process of utilizing high-temperature geothermal water to inhibit the formation of calcium carbonate scale in geothermal wells. Potassium hydroxide solution is added to the generated copolymer to adjust the pH value of the copolymer solution to 5.0, and the copolymer is dried after precipitation with anhydrous methanol and vacuum filtration by a suction pump to obtain a purified scale inhibitor.
[0032] Through experiments, it was found that under the conditions of 150℃~200℃, the scale inhibition rate can reach more than 94%.
[0033] Example 1
[0034] The specific chemical components in geothermal water are shown in Table 1.
[0035] Table 1 Geothermal fluid detection report
[0036]
[0037] In order to solve the problem of calcium carbonate scale adhesion on the surface of geothermal wellbore during the utilization of geothermal water, a high temperature resistant scale inhibitor is required. Table 2 shows the main components of the simulated geothermal fluid obtained according to the geothermal fluid detection report in the geothermal well in Table 1.
[0038] Table 2 Main components of geothermal fluid simulated in Boye area
[0039]
[0040]
[0041] (1) Preparation of scale inhibitor, the method is as follows:
[0042] The first step is to prepare a three-necked flask, with a thermometer placed in the first neck for real-time detection of temperature changes in the flask, a separatory funnel placed in the second neck for adding an initiator, and a reflux condenser placed in the third neck for reflux condensation of organic matter; five monomers, namely acrylic acid (AA), hydroxyethyl methacrylate (HEMA), sodium allyl sulfonate (SAS), citric acid (CA) and sodium glutamate (MSG), are placed in the three-necked flask, wherein the mass ratio of acrylic acid, hydroxyethyl methacrylate, sodium allyl sulfonate, citric acid and sodium glutamate is 32:4:4:2:3;
[0043] In the second step, tert-butanol having a mass ratio of 10% to the total mass of the five monomers is placed in the three-necked flask in the first step, and then deionized water is added to completely dissolve the tert-butanol in the deionized water. The tert-butanol has a purity of 99% and serves as a molecular weight regulator for the reaction.
[0044] The third step is to place the three-necked flask in a magnetic stirring heater preheated to 30°C for water bath heating, and then adjust the temperature of the magnetic stirring heater to 80°C for constant temperature heating;
[0045] In the fourth step, an ammonium persulfate initiator solution with a mass concentration of 7.27% is poured into a separatory funnel, wherein the mass ratio of the ammonium persulfate in the ammonium persulfate initiator solution to the total mass of the five monomers is 1:10; and then the separatory funnel knob is adjusted so that the ammonium persulfate solution is dripped into the reaction solution at a drip rate of one drop every three to five seconds to ensure the stability and full progress of the reaction. After three hours of constant temperature heating, the three-necked flask is taken out and cooled to 25°C. The obtained copolymer is the scale inhibitor AA-HEMA-SAS-CA-MSG required for inhibiting the formation of calcium carbonate scale in geothermal wells during the utilization of high-temperature geothermal water. Potassium hydroxide solution is added to the generated copolymer to adjust the pH value of the copolymer solution to 5.0, and the copolymer is dried after precipitation with anhydrous methanol and vacuum filtration by a suction pump to obtain a purified scale inhibitor.
[0046] (2) According to the main components of geothermal fluid in Table 2, simulated geothermal water was prepared, and the AA-HEMA-SAS-CA-MSG new scale inhibitor prepared in (1) was added to the test solution at 12 mg / L. A static scale inhibition test was carried out in accordance with GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method".
[0047] The static scale inhibition rate of the new AA-HEMA-SAS-CA-MSG scale inhibitor for CaCO3 is 98.13%.
[0048] Example 2
[0049] (1) The mass ratio of the five monomers of acrylic acid (AA), hydroxyethyl methacrylate (HEMA), sodium allyl sulfonate (SAS), citric acid (CA) and sodium glutamate (MSG) in Example 1 was replaced to 40:3:3:1:2, the water bath heating temperature in the magnetic stirring heater was replaced to 50° C., and the cooling temperature was replaced to 28° C., and the scale inhibitor AA-HEMA-SAS-CA-MSG was prepared according to the method for preparing the scale inhibitor in Example 1;
[0050] (2) According to the main components of geothermal fluid in Table 2, simulated geothermal water was prepared, and the AA-HEMA-SAS-CA-MSG novel scale inhibitor prepared in (1) was added to the test solution at 12 mg / L, and a static scale inhibition experiment was performed with reference to GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method". The static scale inhibition rate of the AA-HEMA-SAS-CA-MSG novel scale inhibitor for CaCO3 was measured to be 96.23%.
[0051] Example 3
[0052] (1) The mass ratio of the five monomers of acrylic acid (AA), hydroxyethyl methacrylate (HEMA), sodium allyl sulfonate (SAS), citric acid (CA) and sodium glutamate (MSG) in Example 1 was replaced to 60:3:4:1:5, the water bath heating temperature in the magnetic stirring heater was replaced to 40° C., and the cooling temperature was replaced to 28° C., and the scale inhibitor AA-HEMA-SAS-CA-MSG was prepared according to the method for preparing the scale inhibitor in Example 1;
[0053] (2) According to the main components of geothermal fluid in Table 2, simulated geothermal water was prepared, and the AA-HEMA-SAS-CA-MSG novel scale inhibitor prepared in (1) was added to the test solution at 12 mg / L, and a static scale inhibition test was performed with reference to GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method". The static scale inhibition rate of the AA-HEMA-SAS-CA-MSG novel scale inhibitor for CaCO3 was measured to be 98.84%.
[0054] Example 4
[0055] (1) The mass ratio of the five monomers of acrylic acid (AA), hydroxyethyl methacrylate (HEMA), sodium allyl sulfonate (SAS), citric acid (CA) and sodium glutamate (MSG) in Example 1 was replaced to 32:6:3:2:2, the water bath heating temperature in the magnetic stirring heater was replaced to 60° C., and the cooling temperature was replaced to 30° C., and the scale inhibitor AA-HEMA-SAS-CA-MSG was prepared according to the method for preparing the scale inhibitor in Example 1;
[0056] (2) According to the main components of geothermal fluid in Table 2, simulated geothermal water was prepared, and the AA-HEMA-SAS-CA-MSG novel scale inhibitor prepared in (1) was added to the test solution at 12 mg / L, and a static scale inhibition experiment was performed with reference to GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method". The static scale inhibition rate of the AA-HEMA-SAS-CA-MSG novel scale inhibitor for CaCO3 was measured to be 95.03%.
[0057] Example 5
[0058] (1) The mass ratio of the five monomers of acrylic acid (AA), hydroxyethyl methacrylate (HEMA), sodium allyl sulfonate (SAS), citric acid (CA) and sodium glutamate (MSG) in Example 1 was replaced to 32:4:7:1:2, the water bath heating temperature in the magnetic stirring heater was replaced to 80° C., and the cooling temperature was replaced to 26° C., and the scale inhibitor AA-HEMA-SAS-CA-MSG was prepared according to the method for preparing the scale inhibitor in Example 1;
[0059] (2) According to the main components of geothermal fluid in Table 2, simulated geothermal water was prepared, and the AA-HEMA-SAS-CA-MSG novel scale inhibitor prepared in (1) was added to the test solution at 12 mg / L, and a static scale inhibition experiment was performed with reference to GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method". The static scale inhibition rate of the AA-HEMA-SAS-CA-MSG novel scale inhibitor for CaCO3 was measured to be 93.13%.
[0060] Example 6
[0061] (1) The mass ratio of the five monomers of acrylic acid (AA), hydroxyethyl methacrylate (HEMA), sodium allyl sulfonate (SAS), citric acid (CA) and sodium glutamate (MSG) in Example 1 was replaced with 32:7:6:3:2, the water bath heating temperature in the magnetic stirring heater was replaced with 70° C., and the cooling temperature was replaced with 27° C., and the scale inhibitor AA-HEMA-SAS-CA-MSG was prepared according to the method for preparing the scale inhibitor in Example 1;
[0062] (2) According to the main components of geothermal fluid in Table 2, simulated geothermal water was prepared, and the AA-HEMA-SAS-CA-MSG novel scale inhibitor prepared in (1) was added to the test solution at 12 mg / L, and a static scale inhibition experiment was performed with reference to GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method". The static scale inhibition rate of the AA-HEMA-SAS-CA-MSG novel scale inhibitor for CaCO3 was measured to be 93.22%.
[0063] Example 7
[0064] (1) The mass ratio of the five monomers of acrylic acid (AA), hydroxyethyl methacrylate (HEMA), sodium allyl sulfonate (SAS), citric acid (CA) and sodium glutamate (MSG) in Example 1 was replaced with 32:7:6:3:7, the water bath heating temperature in the magnetic stirring heater was replaced with 80° C., and the cooling temperature was replaced with 29° C., and the scale inhibitor AA-HEMA-SAS-CA-MSG was prepared according to the method for preparing the scale inhibitor in Example 1;
[0065] (2) According to the main components of geothermal fluid in Table 2, simulated geothermal water was prepared, and the AA-HEMA-SAS-CA-MSG novel scale inhibitor prepared in (1) was added to the test solution at 12 mg / L, and a static scale inhibition experiment was performed with reference to GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method". The static scale inhibition rate of the AA-HEMA-SAS-CA-MSG novel scale inhibitor for CaCO3 was measured to be 92.77%.
[0066] Example 8
[0067] (1) The mass ratio of the five monomers of acrylic acid (AA), hydroxyethyl methacrylate (HEMA), sodium allyl sulfonate (SAS), citric acid (CA) and sodium glutamate (MSG) in Example 1 was replaced to 32:3:3:4:2, the water bath heating temperature in the magnetic stirring heater was replaced to 70° C., and the cooling temperature was replaced to 27° C., and the scale inhibitor AA-HEMA-SAS-CA-MSG was prepared according to the method for preparing the scale inhibitor in Example 1;
[0068] (2) According to the main components of geothermal fluid in Table 2, simulated geothermal water was prepared, and the AA-HEMA-SAS-CA-MSG novel scale inhibitor prepared in (1) was added to the test solution at 12 mg / L, and a static scale inhibition experiment was performed with reference to GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method". The static scale inhibition rate of the AA-HEMA-SAS-CA-MSG novel scale inhibitor for CaCO3 was measured to be 91.60%.
[0069] Example 9
[0070] (1) The mass ratio of the five monomers of acrylic acid (AA), hydroxyethyl methacrylate (HEMA), sodium allyl sulfonate (SAS), citric acid (CA) and sodium glutamate (MSG) in Example 1 was replaced to 32:3:3:2:6, the water bath heating temperature in the magnetic stirring heater was replaced to 40° C., and the cooling temperature was replaced to 27° C., and the scale inhibitor AA-HEMA-SAS-CA-MSG was prepared according to the method for preparing the scale inhibitor in Example 1;
[0071] (2) According to the main components of geothermal fluid in Table 2, simulated geothermal water was prepared, and the AA-HEMA-SAS-CA-MSG novel scale inhibitor prepared in (1) was added to the test solution at 12 mg / L, and a static scale inhibition experiment was performed with reference to GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method". The static scale inhibition rate of the AA-HEMA-SAS-CA-MSG novel scale inhibitor for CaCO3 was measured to be 87.59%.
[0072] Example 10
[0073] (1) Prepare the scale inhibitor AA-HEMA-SAS-CA-MSG according to the method for preparing the scale inhibitor in Example 1;
[0074] (2) According to the main components of geothermal fluid in Table 2, simulated geothermal water was prepared, and the AA-HEMA-SAS-CA-MSG novel scale inhibitor prepared in (1) was added to the test solution at 12 mg / L, and a static scale inhibition experiment was performed with reference to GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method". The difference from Example 1 is that the set temperature is 130°C when determining the scale inhibition rate of the composite scale inhibitor for calcium carbonate. The static scale inhibition rate of the AA-HEMA-SAS-CA-MSG novel scale inhibitor for CaCO3 was measured to be 95.43%.
[0075] Embodiment 11
[0076] (1) Prepare the scale inhibitor AA-HEMA-SAS-CA-MSG according to the method for preparing the scale inhibitor in Example 1;
[0077] (2) According to the main components of geothermal fluid in Table 2, simulated geothermal water was prepared, and the AA-HEMA-SAS-CA-MSG novel scale inhibitor prepared in (1) was added to the test solution at 12 mg / L, and a static scale inhibition experiment was performed with reference to GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method". The difference from Example 1 is that the set temperature is 150°C when determining the scale inhibition rate of the composite scale inhibitor for calcium carbonate. The static scale inhibition rate of the AA-HEMA-SAS-CA-MSG novel scale inhibitor for CaCO3 was measured to be 96.21%.
[0078] Example 12
[0079] (1) Prepare the scale inhibitor AA-HEMA-SAS-CA-MSG according to the method for preparing the scale inhibitor in Example 1;
[0080] (2) According to the main components of geothermal fluid in Table 2, simulated geothermal water was prepared, and the AA-HEMA-SAS-CA-MSG novel scale inhibitor prepared in (1) was added to the test solution at 12 mg / L, and a static scale inhibition experiment was performed with reference to GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method". The difference from Example 1 is that the set temperature is 170°C when determining the scale inhibition rate of the composite scale inhibitor for calcium carbonate. The static scale inhibition rate of the AA-HEMA-SAS-CA-MSG novel scale inhibitor for CaCO3 was measured to be 97.27%.
[0081] Embodiment 13
[0082] (1) Prepare the scale inhibitor AA-HEMA-SAS-CA-MSG according to the method for preparing the scale inhibitor in Example 1;
[0083] (2) According to the main components of geothermal fluid in Table 2, simulated geothermal water was prepared, and the AA-HEMA-SAS-CA-MSG novel scale inhibitor prepared in (1) was added to the test solution at 12 mg / L, and a static scale inhibition experiment was performed with reference to GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method". The difference from Example 1 is that the set temperature is 200°C when determining the scale inhibition rate of the composite scale inhibitor for calcium carbonate. The static scale inhibition rate of the AA-HEMA-SAS-CA-MSG novel scale inhibitor for CaCO3 was measured to be 94.68%.
[0084] Embodiment 14
[0085] (1) The scale inhibitor AA-HEMA-SAS-CA-MSG was prepared according to the method for preparing the scale inhibitor in Example 1.
[0086] (2) According to the main components of geothermal fluid in Table 2, simulated geothermal water was prepared, and the AA-HEMA-SAS-CA-MSG novel scale inhibitor prepared in (1) was added to the test solution at 12 mg / L, and a static scale inhibition experiment was performed with reference to GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method". The difference from Example 1 is that the set temperature is 210°C when determining the scale inhibition rate of the composite scale inhibitor for calcium carbonate. The static scale inhibition rate of the AA-HEMA-SAS-CA-MSG novel scale inhibitor for CaCO3 was measured to be 94.11%.
[0087] Comparative Example 1
[0088] (1) This comparative example uses the green and environmentally friendly scale and corrosion inhibitor PASP for comparison. The difference from Example 9 is that an equal amount of PASP is used to replace the new scale inhibitor AA-HEMA-SAS-CA-MSG.
[0089] (2) The static scale inhibition rate of the green and environmentally friendly scale and corrosion inhibitor PASP against CaCO3 was measured to be 76.67%.
[0090] Comparative Example 2
[0091] (1) This comparative example uses the green and environmentally friendly scale and corrosion inhibitor PAA for comparison. The difference from Example 9 is that an equal amount of PAA is used to replace the new scale inhibitor AA-HEMA-SAS-CA-MSG.
[0092] (2) The static scale inhibition rate of the green and environmentally friendly scale and corrosion inhibitor PAA on CaCO3 was measured to be 53.26%.
[0093] Comparative Example 3
[0094] (1) This comparative example uses the green and environmentally friendly scale and corrosion inhibitor PESA for comparison. The difference from Example 9 is that an equal amount of PESA is used to replace the new scale inhibitor AA-HEMA-SAS-CA-MSG.
[0095] (2) The static scale inhibition rate of green and environmentally friendly scale and corrosion inhibitor PESA on CaCO3 was measured to be 46.17%.
[0096] Comparative Example 4
[0097] (1) This comparative example uses the green and environmentally friendly scale and corrosion inhibitor HPMA for comparison. The difference from Example 9 is that an equal amount of HPMA is used to replace the new scale inhibitor AA-HEMA-SAS-CA-MSG.
[0098] (2) The static scale inhibition rate of the green and environmentally friendly scale and corrosion inhibitor HPMA on CaCO3 was measured to be 61.37%.
[0099] Comparative Example 5
[0100] (1) This comparative example uses a commercial green and environmentally friendly scale inhibitor for comparison. The difference from Example 9 is that an equal amount of commercial green and environmentally friendly scale inhibitor is used to replace the AA-HEMA-SAS-CA-MSG novel scale inhibitor.
[0101] (2) The static scale inhibition rate of commercial green and environmentally friendly scale and corrosion inhibitor for CaCO3 was measured to be 69.56%.
[0102] like Figure 2 As shown in the figure, the static scale inhibition rate of the new AA-HEMA-SAS-CA-MSG scale inhibitor for CaCO3 is above 94% in the temperature range of 50-200°C. It is higher than the scale inhibition rate of general scale inhibitors, while other scale inhibitors (such as polyacrylic acid (PAA), polyaspartic acid (PASP), polyepoxysuccinic acid (PESA), hydrolyzed polymaleic acid (HPMA) and commercial scale inhibitors) have different scale inhibition rates at different temperatures, but the basic scale inhibition rates are not very stable.
[0103] It is worth noting that although the preferred embodiments of the present invention have been described in detail above in conjunction with the accompanying drawings, the present invention is not limited to the above-mentioned specific implementation methods. The above-mentioned implementation methods are merely illustrative and not restrictive. Relevant technical personnel in the field can be inspired by the present invention and make many forms without departing from the purpose of the present invention and the scope of protection of the claims, which all belong to the scope of protection of the present invention.
Claims
1. A method for preparing a scale inhibitor for inhibiting the formation of calcium carbonate scale in geothermal wells during the utilization of high-temperature geothermal water, characterized in that: The components of high-temperature geothermal water include: NaCO3 13.74mmol / L, NaF 0.44mmol / L, NaI 0.01mmol / L, NaSO4 2.18mmol / L, CaCl24.42mmol / L, MgCl2 1.65mmol / L, NaCl 54.92mmol / L and KCl 3.82mmol / L; Processing the high-temperature geothermal water comprises the following steps: The first step is to prepare a three-necked flask, wherein a thermometer is placed at the first neck to detect the temperature change in the flask in real time, a separatory funnel is placed at the second neck to add an initiator, and a reflux condenser is placed at the third neck to reflux and condense organic matter; five monomers, namely acrylic acid, hydroxyethyl methacrylate, sodium allyl sulfonate, citric acid and sodium glutamate, are placed in the three-necked flask, wherein the mass ratio of acrylic acid, hydroxyethyl methacrylate, sodium allyl sulfonate, citric acid and sodium glutamate is (32-60):(4-7):(4-7):(2-4):(3-7); In the second step, tert-butanol having a mass ratio of 10% to the total mass of the five monomers is placed in the three-necked flask in the first step, and then deionized water is added to completely dissolve the tert-butanol in the deionized water. The mass fraction of the tert-butanol is 99%, which serves as a molecular weight regulator for the reaction. The third step is to place the three-necked flask in a magnetic stirring heater that has been preheated to a temperature between 30°C and 80°C for water bath heating, and after adjusting the temperature of the magnetic stirring heater to 80°C, perform constant temperature heating; The fourth step is to pour an ammonium persulfate initiator solution with a mass percentage concentration of 7.27% into a separatory funnel, wherein the mass ratio of the ammonium persulfate in the ammonium persulfate initiator solution to the total mass of the five monomers is 1:10; then adjust the knob of the separatory funnel to drip the ammonium persulfate solution into the reaction solution at a dripping rate of one drop every three to five seconds; after constant temperature heating for three hours, take out the three-necked flask and cool it to between 25°C and 30°C. The obtained copolymer is the scale inhibitor AA-HEMA-SAS-CA-MSG for inhibiting the formation of calcium carbonate scale in geothermal wells during the utilization of high-temperature geothermal water; potassium hydroxide solution is added to the generated copolymer to adjust the pH value of the copolymer solution to 5.0; the copolymer is precipitated with anhydrous methanol, and the copolymer is dried after vacuum filtration by a suction pump to obtain a purified scale inhibitor; the scale inhibitor AA-HEMA-SAS-CA-MSG chelates with calcium ions in the geothermal fluid, thereby inhibiting the formation of calcium carbonate scale in the geothermal fluid.
Citation Information
Patent Citations
Terpolymer scale inhibitor and preparation method thereof
CN108147559A
Calcium carbonate scale inhibitor and preparation method thereof
CN110845664A
Ternary scale inhibitor and preparation method thereof
CN112225843A