Nanoimprint template glue and preparation method thereof
By using components such as epoxy modified polysiloxane resin in nanoimprinted template glue, combined with cationic/radical hybrid deep curing technology, the problems of high curing volume shrinkage and poor mechanical properties are solved, and low The shrinkage rate and high mechanical strength ensure high precision and high resolution imprinting effect.
Patent Information
- Application Number
- CN202211686239.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-12-27
AI Technical Summary
The existing nanoimprint template glue has a large volume shrinkage rate during the curing process, poor mechanical properties, and is prone to breaking the residual glue, affecting the quality and service life of the imprint, and it is difficult to make high-precision and high-resolution graphics.
Using epoxy modified polysiloxane resin, silicone fluorine modified polyurethane acrylic resin, fluorine modified acrylic esters, modified epoxy acrylic resin, cationic hybrid acrylic resin, crosslinked diluents and flexible chain extenders, etc. Through cationic/radical hybrid deep curing technology, the curing volume shrinkage rate is reduced, and the mechanical strength and mold release efficiency are improved.
The volume shrinkage rate after curing is achieved by less than 3%, improving mechanical strength and toughness, ensuring complete demolding after multiple imprints, and enhancing the accuracy and service life of the imprinted pattern.
Smart Images

Figure BDA0004021100390000021 
Figure BDA0004021100390000041 
Figure BDA0004021100390000051
Abstract
Description
Technical Field
[0001] The invention relates to the field of materials, and in particular to a nanoimprint template glue and a preparation method thereof. Background Art
[0002] In nanoimprint lithography (NIL), the template is the biggest difference between imprint lithography and traditional optical lithography. As the initial carrier of imprint features, the template directly determines the quality of the imprint pattern. To achieve high-quality imprint replicas, a high-quality imprint template is required. Unlike the mask (4X) used in traditional optical lithography, nanoimprint lithography uses a 1X template, which faces greater challenges in template production, inspection and repair technology.
[0003] Currently, many research teams are committed to the study of soft templates. Soft templates generally refer to templates whose substrates are made of soft materials. Usually, photoresist is used as a prepolymer, and patterns are made on its surface using imprinting technology. Then, the soft templates are formed by thermal curing or UV curing to obtain polymer soft templates that can replicate the patterns in reverse. Compared with hard templates, soft templates not only have a simple preparation process and greatly save costs, but also can compensate for surface morphology differences, which can replace the disadvantage of hard materials that cannot be bent, greatly improving the quality of imprinting and the area of imprinted patterns.
[0004] Currently, most nanoimprint template glues are acrylic polymers, which use UV-curing free radical polymerization. They can be quickly cured after UV irradiation, but the glue layer shrinks greatly after curing, with a volume shrinkage rate of 6% to 10%, which seriously causes changes in the size of the microstructure after imprinting; the mechanical properties of the polymer film layer are relatively poor, and the residual glue is easily broken during the imprinting and demolding process, resulting in structural defects; the surface energy increases after multiple imprinting, making it difficult to demold, affecting the service life; the glue shrinks greatly after free radical curing, resulting in differences in structural accuracy, affecting the optical properties of the product after imprinting; it is not wear-resistant, especially for producing high-precision, high-resolution graphics. Summary of the invention
[0005] In view of this, the present invention provides a nanoimprint template adhesive and a preparation method thereof. The nanoimprint template adhesive provided by the present invention can effectively reduce the volume shrinkage during curing, improve the mechanical strength and toughness, improve the demoulding efficiency, and can be completely demoulded after multiple imprinting.
[0006] The present invention provides a nanoimprint template adhesive, which is prepared from raw materials including the following components in mass ratio:
[0007]
[0008] Preferably, the epoxy-modified polysiloxane resin is prepared by the following preparation method:
[0009] Silicone oil is mixed with 4-vinyl cyclohexene oxide to react and obtain epoxy-modified polysiloxane resin.
[0010] Preferably, the mass ratio of the silicone oil to 4-vinyl epoxyhexane is 27.5 to (29.5 to 31);
[0011] The hydrogen content of the silicone oil is 1.5wt% to 1.65wt%;
[0012] The reaction is carried out under the action of a catalyst; the catalyst is a rhodium catalyst; the mass ratio of the catalyst to the silicone oil is (0.095-0.1):100.
[0013] Preferably, the preparation method specifically comprises:
[0014] Silicone oil, 4-vinyl cyclohexene oxide and a catalyst are mixed, stirred at 30-40° C. for 24-36 hours, and then heated to 80-90° C. and stirred for 3-5 hours to obtain an epoxy-modified polysiloxane resin.
[0015] Preferably, the organic silicon fluorine-modified polyurethane acrylic resin is at least one of UV-9843A, UV-9843-1, UV-9843-2, Trust-7760, FSP8658, and LuCure8696.
[0016] Preferably, the fluorine-modified acrylate is at least one of perfluorooctyl ethyl acrylate, dodecafluoroheptyl methacrylate, (N-methylperfluorohexylsulfonamido)ethyl acrylate, perfluorohexyl ethyl acrylate, perfluorohexyl ethyl methacrylate, perfluorobutyl ethyl acrylate and 1H,1H,2H,2H-perfluorooctanol acrylate.
[0017] Preferably, the modified epoxy acrylic resin is at least one of Ebecryl600, Agisyn 6050TF, WORLD ROCK700, 3,4-epoxycyclohexylmethyl methacrylate and neopentyl glycol polymethyl ethylene oxide diacrylate;
[0018] The cationic hybrid acrylic resin is at least one of U-9100A, U-9100B, U-9101, U-9103, U-9200, U-9210, U-9310 and U-9340.
[0019] Preferably, the cross-linking diluent is at least one of hydroxybutyl vinyl ether, triethylene glycol divinyl ether, 1,4-cyclohexyl dimethanol divinyl ether, butyl vinyl ether, 1,6-hexanediol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, tris(2-hydroxyethyl)isocyanuric acid triacrylate, di(trimethylolpropane) tetraacrylate, 4(ethoxylated) pentaerythritol tetraacrylate and pentaerythritol tetraacrylate;
[0020] The flexible chain extender is at least one of 3 (ethoxy) trimethylolpropane triacrylate, 6 (ethoxy) trimethylolpropane triacrylate, 9 (ethoxy) trimethylolpropane triacrylate, 15 (ethoxy) trimethylolpropane triacrylate, and 20 (ethoxy) trimethylolpropane triacrylate;
[0021] The photoinitiator is at least one of photoinitiator 1173, photoinitiator 184, IPO, photoinitiator 127, photoinitiator 369, photoinitiator ITX, photoinitiator BDK and photoinitiator 819;
[0022] The cationic initiator is ANTHRACURE TM UVS-1331、ANTHRACURE TM At least one of UVS-1101, Easepi6992, Easepi 1176 and Easepi 250.
[0023] The present invention also provides a method for preparing the nanoimprint template glue described in the above technical solution, comprising the following steps:
[0024] a) mixing an organosilicon fluorine-modified polyurethane acrylic resin, a modified epoxy acrylic resin, a fluorine-modified acrylate, a cross-linking diluent and a flexible chain extender to obtain a mixed solution 1;
[0025] b) mixing the mixed solution 1 with a photoinitiator, a cationic initiator and a cationic hybrid acrylic resin to obtain a mixed solution 2;
[0026] c) mixing the mixed solution 2 with an epoxy-modified polysiloxane resin to obtain a mixed solution 3;
[0027] d) degassing and sieve filtering the mixed solution 3 to obtain a nanoimprint template glue.
[0028] Preferably, the method specifically comprises the following steps:
[0029] a) adding organic silicon fluorine-modified polyurethane acrylic resin, modified epoxy acrylic resin, fluorine-modified acrylate, cross-linking diluent and flexible chain extender into a container, stirring at a rate of 600-800 r / min for 20-30 min, and then stirring at a rate of 1000-1200 r / min for 20-30 min to obtain a mixed solution 1; during the above process, the liquid temperature in the container is maintained at 10±1°C;
[0030] b) adding a photoinitiator, a cationic initiator and a cationic hybrid acrylic resin into the container, stirring at a rate of 1000 to 1200 r / min for 30 to 40 min to obtain a mixed solution 2; during the above process, the liquid temperature in the container is maintained at 10±1° C.;
[0031] c) adding epoxy-modified polysiloxane resin into the container, stirring at a rate of 1000 to 1200 r / min for 30 to 40 min to obtain a mixed solution 3;
[0032] d) degassing and sieve filtering the mixed solution 3 to obtain a nanoimprint template glue.
[0033] The nanoimprint template glue provided by the present invention is prepared by mixing epoxy-modified polysiloxane resin, silicone-fluorine-modified polyurethane acrylic resin, fluorine-modified acrylate, modified epoxy acrylic resin, cationic hybrid acrylic resin, cross-linking diluent, flexible chain extender, photoinitiator and cationic initiator in a certain proportion. The present invention introduces epoxy-modified polysiloxane resin, fluorine-modified flexible acrylic resin, fluorine-modified epoxy acrylic resin, cationic hybrid acrylic polymer and the like into the structure through molecular design, so that the template glue has the characteristics of high mechanical strength, good demoulding performance, long service life and the like. At the same time, in addition to the acrylate containing carbon-carbon double bonds, the main resin of the present invention also contains epoxy groups that can realize cationic ring-opening curing. With the assistance of auxiliary curing materials, free radical / cationic hybrid deep curing can be quickly realized by UV. Compared with the existing template glue, the curing volume shrinkage rate of the glue can be reduced to less than 3%, and the size change is very small. That is, the present invention adopts cationic / free radical hybrid fluorine-modified epoxy acrylic resin as the main raw material of the adhesive. The molecular structure of the resin contains epoxy groups, double bond groups and low surface energy fluorine groups at the same time. During the light curing process, the system combines the curing shrinkage and curing rate, and can achieve deep ultra-low shrinkage cationic / free radical composite UV curing, greatly reduce the shrinkage, can quickly demold, and realize multiple precision imprinting.
[0034] The test results show that the template glue obtained by the present invention has an appearance of a colorless to light yellow transparent liquid, a viscosity of 400-500mPa.s, and good fluidity; after curing, the hardness reaches below 90A, the tensile strength reaches above 6.5MPa, and the Young's modulus reaches above 50MPa, showing excellent toughness and mechanical strength; the volume shrinkage rate after curing is below 3%, showing ultra-low shrinkage; the surface water drop angle of the newly made template reaches above 115°, the surface energy is low, and continuous imprinting is performed for multiple times, and the demolding can be completed, thereby improving the demolding efficiency. DETAILED DESCRIPTION
[0035] The present invention provides a nanoimprint template adhesive, which is prepared from raw materials including the following components in mass ratio:
[0036]
[0037]
[0038] The raw materials for preparing the nano-imprint template glue of the present invention include: epoxy-modified polysiloxane resin.
[0039] In the present invention, the epoxy-modified polysiloxane resin is preferably prepared by the following preparation method: silicone oil and 4-vinyl cyclohexene oxide are mixed and reacted to obtain the epoxy-modified polysiloxane resin.
[0040] in:
[0041] The silicone oil is preferably PHMS silicone oil, and the hydrogen content of the silicone oil is preferably 1.5wt% to 1.65wt%, specifically 1.5wt%, 1.55%, 1.6%, 1.65%. The source of the silicone oil is not particularly limited, and it can be a commercial product.
[0042] The source of the 4-vinylcyclohexene oxide is not particularly limited and may be a commercial product.
[0043] The mass ratio of the silicone oil to 4-vinyl cyclohexene oxide is preferably 27.5:(29.5-31), specifically 27.5:29.5, 27.5:30, 27.5:30.5, 27.7:31.
[0044] The reaction is preferably carried out under the action of a catalyst. The catalyst is preferably a rhodium catalyst. The mass ratio of the catalyst to the silicone oil is preferably (0.095-0.1):100, specifically 0.095:100, 0.098:100, 0.1:100.
[0045] The temperature conditions of the mixed reaction are preferably: first stirring at 30-40°C, specifically 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C, 40°C. The stirring rate is preferably 500-600rpm, specifically 500rpm, 550rpm, 600rpm. The stirring time is preferably 24-36h, specifically 24h, 25h, 26h, 28h, 30h, 32h, 34h, 36h. Stirring at the above temperature until the catalyst is completely dissolved. Then heating to 80-90°C and continuing stirring, specifically 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, 90°C. The stirring rate is preferably 500-600rpm, specifically 500rpm, 550rpm, 600rpm. The stirring time is preferably 3 to 5 hours, specifically 3 hours, 4 hours, or 5 hours. After the above mixing reaction, an epoxy-modified polysiloxane resin is obtained.
[0046] In the present invention, the specific process of the above preparation method preferably includes: mixing silicone oil, 4-vinyl cyclohexene oxide and a catalyst, stirring at 30-40°C for 24-36 hours, and then heating to 80-90°C and stirring for 3-5 hours to obtain an epoxy-modified polysiloxane resin. The specific values of the temperature, stirring conditions, etc. of each step are consistent with those described above and are not repeated here. The silicone oil, 4-vinyl cyclohexene oxide and a catalyst are mixed, and after the catalyst is completely dissolved, they are stirred at 30-40°C.
[0047] In the present invention, the mass ratio of the epoxy-modified polysiloxane resin in the raw materials for preparing the nanoimprint template glue is 10% to 25%, specifically 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%.
[0048] The raw materials for preparing the nanoimprint template glue of the present invention also include: organic silicon fluorine modified polyurethane acrylic resin.
[0049] In the present invention, the organic silicon fluorine-modified polyurethane acrylic resin is preferably at least one of UV-9843A, UV-9843-1, UV-9843-2, Trust-7760, FSP8658, and LuCure8696; wherein UV-9843A, UV-9843-1, and UV-9843-2 are derived from Dongguan Inoue New Materials, Trust-7760 is derived from Shenzhen Youyang Technology Co., Ltd., and FSP8658 is derived from Runao Chemical.
[0050] In the present invention, the mass ratio of the organic silicon fluorine-modified polyurethane acrylic resin in the raw materials for preparing the nanoimprint template glue is 20% to 30%, specifically 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%.
[0051] The raw materials for preparing the nanoimprint template glue of the present invention also include: fluorine-modified acrylate.
[0052] In the present invention, the fluorine-modified acrylate is preferably at least one of perfluorooctyl ethyl acrylate, dodecafluoroheptyl methacrylate, (N-methylperfluorohexylsulfonamido)ethyl acrylate, perfluorohexyl ethyl acrylate, perfluorohexyl ethyl methacrylate, perfluorobutyl ethyl acrylate and 1H,1H,2H,2H-perfluorooctanol acrylate. The present invention has no particular restrictions on the source of the fluorine-modified acrylate, and it can be a commercial product.
[0053] In the present invention, the mass ratio of the fluorine-modified acrylate in the raw materials for preparing the nanoimprint template glue is 15% to 25%, specifically 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%.
[0054] The raw materials for preparing the nanoimprint template glue of the present invention also include: modified epoxy acrylic resin.
[0055] In the present invention, the modified epoxy acrylic resin is preferably at least one of Ebecryl600, Agisyn 6050TF, WORLDROCK 700, 3,4-epoxycyclohexylmethyl methacrylate and neopentyl glycol polymethyl oxirane diacrylate. The present invention has no particular limitation on the source of the modified epoxy acrylic resin, and it can be a commercial product.
[0056] In the present invention, the mass ratio of the modified epoxy acrylic resin in the raw materials for preparing the nanoimprint template adhesive is 5% to 10%, specifically 5%, 6%, 7%, 8%, 9%, or 10%.
[0057] The raw materials for preparing the nanoimprint template glue of the present invention also include: cationic hybrid acrylic resin.
[0058] In the present invention, the cationic hybrid acrylic resin is a cationic hybrid UV resin, preferably at least one of U-9100A, U-9100B, U-9101, U-9103, U-9200, U-9210, U-9310 and U-9340. The present invention has no particular limitation on the source of the cationic hybrid acrylic resin, and it can be a commercial product.
[0059] In the present invention, the mass ratio of the cationic hybrid acrylic resin in the raw materials for preparing the nanoimprint template glue is 12% to 25%, specifically 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 21.5%, 22%, 23%, 24%, 25%.
[0060] The raw materials for preparing the nanoimprint template glue of the present invention also include: a cross-linking diluent.
[0061] In the present invention, the cross-linking diluent is an active diluent, which is a diluent with a cross-linking effect, that is, a type of additive that acts as a diluent and a cross-linking agent at the same time. In the present invention, the cross-linking diluent is preferably hydroxybutyl vinyl ether (HBVE), triethylene glycol divinyl ether (DVE-3), 1,4-cyclohexyl dimethanol divinyl ether (CHVE), butyl vinyl ether (BVE), 1,6-hexanediol diacrylate (HDDA), dipropylene glycol diacrylate (DPGDA), tripropylene glycol diacrylate (TPGDA), trimethylolpropane triacrylate, pentaerythritol triacrylate, tris (2-hydroxyethyl) isocyanuric acid triacrylate, di (trimethylolpropane) tetraacrylate, 4 (ethoxylated) pentaerythritol tetraacrylate and at least one of pentaerythritol tetraacrylate. The present invention has no special restrictions on the source of the cross-linking diluent, and it can be a commercially available commercial product.
[0062] In the present invention, the mass ratio of the cross-linking diluent in the raw materials for preparing the nanoimprint template glue is 3% to 5%, specifically 3%, 4%, or 5%.
[0063] The raw materials for preparing the nanoimprint template glue of the present invention also include: a flexible chain extender.
[0064] In the present invention, the flexible chain extender is preferably 3 (ethoxy) trimethylolpropane triacrylate (i.e., TMP (EO) 3TA), 6 (ethoxy) trimethylolpropane triacrylate (i.e., TMP (EO) 6TA), 9 (ethoxy) trimethylolpropane triacrylate (i.e., TMP (EO) 9TA), 15 (ethoxy) trimethylolpropane triacrylate (i.e., TMP (EO) 15 TA), 20 (ethoxy) trimethylolpropane triacrylate (ie TMP (EO) 20 TA). Among them, 3 (ethoxy) trimethylolpropane triacrylate is also called (3 ethoxy) trimethylolpropane triacrylate, and the names of the other substances are similar. The present invention has no special restrictions on the source of the flexible chain extender, which can be a commercial product, such as that provided by Guangdong Yuhe New Materials Co., Ltd.
[0065] In the present invention, the mass ratio of the flexible chain extender in the raw materials for preparing the nanoimprint template glue is 1% to 3%, specifically 1%, 2%, or 3%.
[0066] The raw materials for preparing the nanoimprint template glue of the present invention also include: a photoinitiator.
[0067] In the present invention, the photoinitiator is preferably at least one of photoinitiator 1173, photoinitiator 184, IPO, photoinitiator 127, photoinitiator 369, photoinitiator ITX, photoinitiator BDK and photoinitiator 819. The present invention has no particular limitation on the source of the photoinitiator, and it can be a commercial product.
[0068] In the present invention, the mass ratio of the photoinitiator in the raw materials for preparing the nanoimprint template glue is 1% to 3%, specifically 1%, 1.5%, 2%, 2.5%, or 3%.
[0069] The raw materials for preparing the nanoimprint template glue of the present invention also include: a cationic initiator.
[0070] In the present invention, the cationic initiator is preferably ANTHRACURE TM UVS-1331、ANTHRACURE TM At least one of UVS-1101, Easepi 6992, Easepi 1176 and Easepi 250. The present invention has no particular limitation on the source of the cationic initiator, and any commercial product may be used.
[0071] In the present invention, the mass ratio of the cationic initiator in the raw materials for preparing the nanoimprint template glue is 1% to 2%, specifically 1%, 1.5%, or 2%.
[0072] The nanoimprint template glue provided by the present invention has a viscosity of 400-500 mPa.s at 25° C., specifically 400 mPa.s, 410 mPa.s, 420 mPa.s, 430 mPa.s, 440 mPa.s, 450 mPa.s, 460 mPa.s, 470 mPa.s, 480 mPa.s, 490 mPa.s, and 500 mPa.s.
[0073] The present invention also provides a method for preparing the nanoimprint template glue described in the above technical solution, comprising the following steps:
[0074] a) mixing an organosilicon fluorine-modified polyurethane acrylic resin, a modified epoxy acrylic resin, a fluorine-modified acrylate, a cross-linking diluent and a flexible chain extender to obtain a mixed solution 1;
[0075] b) mixing the mixed solution 1 with a photoinitiator, a cationic initiator and a cationic hybrid acrylic resin to obtain a mixed solution 2;
[0076] c) mixing the mixed solution 2 with an epoxy-modified polysiloxane resin to obtain a mixed solution 3;
[0077] d) degassing and sieve filtering the mixed solution 3 to obtain a nanoimprint template glue.
[0078] Among them, the types and amounts of silicone fluorine-modified polyurethane acrylic resin, modified epoxy acrylic resin, fluorine-modified acrylate, cross-linking diluent, flexible chain extender, photoinitiator, cationic initiator, cationic hybrid acrylic resin and epoxy-modified polysiloxane resin are consistent with those described in the previous technical solution and will not be repeated here.
[0079] In the present invention, the step a) preferably comprises: adding organic silicon fluorine-modified polyurethane acrylic resin, modified epoxy acrylic resin, fluorine-modified acrylate, cross-linking diluent and flexible chain extender into a container, stirring at a rate of 600 to 800 r / min for 20 to 30 min, and then stirring at a rate of 1000 to 1200 r / min for 20 to 30 min to obtain a mixed solution 1; during the above process, the liquid temperature in the container is maintained at 10±1°C.
[0080] Specifically, after adding the above 6 materials into the container, the sealed container is first slowly stirred at a rate of 600-800r / min for 20-30min to disperse the resin; the stirring rate can be specifically 600r / min, 700r / min, 800r / min; the stirring time can be specifically 20min, 21min, 22min, 23min, 24min, 25min, 26min, 27min, 28min, 29min, 30min. After the above slow stirring, the stirring rate is increased to stir at a rate of 1000-1200r / min for 30-40min; wherein the stirring rate can be specifically 1000r / min, 1100r / min, 1200r / min; the stirring time can be specifically 30min, 31min, 32min, 33min, 34min, 35min, 36min, 37min, 38min, 39min, 40min. During the whole process, the temperature of the liquid in the container is maintained at 10±1° C. After the above mixing treatment, a mixed solution 1 is obtained.
[0081] In the present invention, the step b) preferably comprises: adding a photoinitiator, a cationic initiator and a cationic hybrid acrylic resin into the container, stirring at a rate of 1000 to 1200 r / min for 30 to 40 min to obtain a mixed solution 2; during the above process, the liquid temperature in the container is maintained at 10±1°C.
[0082] Specifically, after the mixed solution 1 is obtained in step a), the photoinitiator, cationic initiator and cationic hybrid acrylic resin are continuously added to the container of step a), and stirred at a rate of 1000-1200 r / min for 30-40 min; the stirring rate can be specifically 1000 r / min, 1100 r / min, 1200 r / min; the stirring time can be specifically 30 min, 31 min, 32 min, 33 min, 34 min, 35 min, 36 min, 37 min, 38 min, 39 min, 40 min. During the above whole process, the liquid temperature in the container is maintained at 10±1°C. After the above mixing treatment, the mixed solution 2 is obtained.
[0083] In the present invention, the step c) preferably comprises: adding epoxy-modified polysiloxane resin into the container, stirring at a rate of 1000 to 1200 r / min for 30 to 40 min, to obtain a mixed solution 3.
[0084] Specifically, after the mixed solution 2 is obtained in step b), epoxy-modified polysiloxane resin is continuously added to the container of step b), and stirred at a rate of 1000-1200 r / min for 30-40 min; the stirring rate can be specifically 1000 r / min, 1100 r / min, 1200 r / min; the stirring time can be specifically 30 min, 31 min, 32 min, 33 min, 34 min, 35 min, 36 min, 37 min, 38 min, 39 min, 40 min. During the above whole process, the liquid temperature in the container is maintained at 10±1°C. After the above mixing treatment, a mixed solution 3 is obtained.
[0085] In the present invention, the step d) preferably comprises: degassing and sieve filtering the mixed solution 3 to obtain a nanoimprint template glue.
[0086] Specifically, after the mixed solution 3 is obtained in step c), vacuum degassing is performed; the vacuum degassing time is preferably 10 to 15 minutes, specifically 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes, and 15 minutes. After degassing, sieve filtration is performed; preferably, 800 to 1000 mesh filter is used for filtration, specifically 800 mesh, 900 mesh, and 1000 mesh. After the above treatment, a nanoimprint template glue is obtained.
[0087] In the preparation method provided by the present invention, in step a), a low-viscosity diluent is used to dilute and dissolve a high-viscosity organosilicon fluorine-modified polyurethane acrylic resin, a modified epoxy acrylic resin and a fluorine-modified acrylate. In step b), an initiator is stirred and dissolved in the diluent. In step c), the epoxy-modified polysiloxane resin is further diluted and dissolved in the diluent.
[0088] The preparation method provided by the present invention mixes 9 kinds of raw materials in steps according to a certain order. Such specific operation steps can quickly dilute and dissolve high-viscosity resin and solid powder initiator to prevent agglomeration and uneven dispersion. If the above mixing order is broken, for example, the epoxy-modified polysiloxane resin in step c) is added to step a), the density of the organosilicon segment in the system will be too large, and it will easily separate from the acrylic resin and be unevenly dispersed. If all 9 kinds of raw materials are directly mixed at one time, it will lead to uneven dispersion.
[0089] The nanoimprint template glue provided by the present invention is prepared by mixing epoxy-modified polysiloxane resin, silicone-fluorine-modified polyurethane acrylic resin, fluorine-modified acrylate, modified epoxy acrylic resin, cationic hybrid acrylic resin, cross-linking diluent, flexible chain extender, photoinitiator and cationic initiator in a certain proportion. The present invention introduces epoxy-modified polysiloxane resin, fluorine-modified flexible acrylic resin, fluorine-modified epoxy acrylic resin, cationic hybrid acrylic polymer and the like into the structure through molecular design, so that the template glue has the characteristics of high mechanical strength, good demoulding performance, long service life and the like. At the same time, in addition to the acrylate containing carbon-carbon double bonds, the main resin of the present invention also contains epoxy groups that can realize cationic ring-opening curing. With the assistance of auxiliary curing materials, free radical / cationic hybrid deep curing can be quickly realized by UV. Compared with the existing template glue, the curing volume shrinkage rate of the glue can be reduced to less than 3%, and the size change is very small. That is, the present invention adopts cationic / free radical hybrid fluorine-modified epoxy acrylic resin as the main raw material of the adhesive. The molecular structure of the resin contains epoxy groups, double bond groups and low surface energy fluorine groups at the same time. During the light curing process, the system combines the curing shrinkage and curing rate, and can achieve deep ultra-low shrinkage cationic / free radical composite UV curing, greatly reduce the shrinkage, can quickly demold, and realize multiple precision imprinting.
[0090] The present invention has the following beneficial effects:
[0091] 1. The template glue is solvent-free, environmentally friendly and safe.
[0092] 2. The viscosity of the template glue is 400-500mPa.s, with good fluidity, easy to apply glue, and no glue overflow during embossing.
[0093] 3. The template glue introduces epoxy modified structure and three-dimensional cross-linked network, and adds flexible chain extender toughening agent to make the colloid have high mechanical strength and toughness, which is convenient for repeated multiple imprinting, and the glue is continuously glued during the imprinting process, and the service life is long. In addition, a large number of fluorine modified groups and polysiloxane structures are introduced into the template glue. After the glue is applied, the molecules are rearranged on the substrate. The part with high surface energy is slowly adsorbed on the substrate surface, and the part with low surface energy is distributed on the surface to form an organic double-layer structure. After curing, the adhesion between the film layer and the substrate is enhanced. At the same time, the static water drop angle of the surface is large and the surface energy is low. The template surface does not need further anti-sticking modification. The demoulding efficiency is high during the imprinting process, and the imprinted pattern is defect-free and the structure is complete. At the same time, more benzene rings and organosilicon groups are introduced into the template glue, which have good matching with epoxy modified structure, fluorine modified group and polysiloxane structure, high refractive index, good light transmittance, and form a firm three-dimensional network structure with strong corrosion resistance, chemical resistance and solvent resistance. In addition, the main raw materials of the glue of the present invention can be matched with a free radical / cationic composite curing system, which greatly reduces the volume shrinkage rate, reduces the curing deformation, can transfer the master template pattern well, and has high dimensional accuracy.
[0094] The test results show that the template glue obtained by the present invention has an appearance of a colorless to light yellow transparent liquid, a viscosity of 400-500mPa.s, and good fluidity; after curing, the hardness reaches below 90A, the tensile strength reaches above 6.5MPa, and the Young's modulus reaches above 50MPa, showing excellent toughness and mechanical strength; the volume shrinkage rate after curing is below 3%, showing ultra-low shrinkage; the surface water drop angle of the newly made template reaches above 115°, the surface energy is low, and continuous imprinting is performed for multiple times, and the demolding can be completed, thereby improving the demolding efficiency.
[0095] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0096] Preparatory Example: Preparation of Epoxy-Modified Polysiloxane Resin
[0097] Add 27.5 g of silicone oil (PHMS, hydrogen content 1.6%), 30 g of 4-vinyl cyclohexene oxide and 27 mg of rhodium catalyst into a 100 mL three-necked flask. After the catalyst is completely dissolved, stir at 35 ° C for 24 h, then raise the temperature to 80 ° C and continue stirring for 5 h to obtain a light yellow transparent liquid, i.e., epoxy-modified polysiloxane resin, which is set aside.
[0098] Example 1
[0099] 1. Raw materials:
[0100] The raw material composition for preparing the nanoimprint template glue is shown in Table 1:
[0101] Table 1: Raw material composition
[0102]
[0103] 2. Preparation process
[0104] a) Add silicone fluorine-modified polyurethane acrylic resin, modified epoxy acrylic resin, fluorine-modified acrylate, cross-linking diluent and flexible chain extender into a 100 mL container, seal and slowly stir at a rate of 600 r / min for 20 min, and after the resin is dispersed, stir at a rate of 1000 r / min for 20 min to obtain a mixed solution 1; during this process, the liquid temperature in the container is maintained at 10±1°C.
[0105] b) Add the photoinitiator, cationic initiator and cationic hybrid acrylic resin into the above container, and continue stirring at a rate of 1000 r / min for 30 min to obtain a mixed solution 2; during this process, the liquid temperature in the container is maintained at 10±1°C.
[0106] c) adding epoxy-modified polysiloxane resin into the container, and continuing to stir at a rate of 1000 r / min for 30 min, during which the liquid temperature in the container is maintained at 10±1° C. Then, vacuum degassing is performed for 10 min, and then filtering is performed with an 800-mesh filter to obtain a nanoimprint template glue.
[0107] Example 2
[0108] 1. Raw materials:
[0109] The raw material composition for preparing the nanoimprint template glue is shown in Table 2:
[0110] Table 2: Raw material composition
[0111]
[0112] 2. Preparation process
[0113] a) Add organic silicon fluorine-modified polyurethane acrylic resin, modified epoxy acrylic resin, fluorine-modified acrylate, cross-linking diluent and flexible chain extender into a 100 mL container, seal and slowly stir at a rate of 800 r / min for 30 min, and after the resin is dispersed, stir at a rate of 1200 r / min for 30 min to obtain a mixed solution 1; during this process, the liquid temperature in the container is maintained at 10±1°C.
[0114] b) Add the photoinitiator, cationic initiator and cationic hybrid acrylic resin into the above container, and continue stirring at a rate of 1200 r / min for 40 min to obtain a mixed solution 2; during this process, the liquid temperature in the container is maintained at 10±1°C.
[0115] c) adding epoxy-modified polysiloxane resin into the container, and continuing to stir at a rate of 1200 r / min for 40 min, during which the liquid temperature in the container is maintained at 10±1° C. Then, vacuum degassing is performed for 15 min, and then filtering is performed with a 1000-mesh filter to obtain a nanoimprint template glue.
[0116] Example 3
[0117] 1. Raw materials:
[0118] The raw material composition for preparing the nanoimprint template glue is shown in Table 3:
[0119] Table 3: Raw material composition
[0120]
[0121] 2. Preparation process
[0122] a) Add organic silicon fluorine-modified polyurethane acrylic resin, modified epoxy acrylic resin, fluorine-modified acrylate, cross-linking diluent and flexible chain extender into a 100 mL container, seal and slowly stir at a rate of 700 r / min for 25 min, and after the resin is dispersed, stir at a rate of 1100 r / min for 25 min to obtain a mixed solution 1; during this process, the liquid temperature in the container is maintained at 10±1°C.
[0123] b) Add the photoinitiator, cationic initiator and cationic hybrid acrylic resin into the above container, and continue stirring at a rate of 1100 r / min for 35 min to obtain a mixed solution 2; during this process, the liquid temperature in the container is maintained at 10±1°C.
[0124] c) adding epoxy-modified polysiloxane resin into the container, and continuing to stir at a rate of 1100 r / min for 35 min, during which the liquid temperature in the container is maintained at 10±1° C. Then, vacuum degassing is performed for 13 min, and then filtering is performed with a 900-mesh filter to obtain a nanoimprint template glue.
[0125] Example 4: Performance Test
[0126] The nanoimprint template adhesives obtained in Examples 1-3 were tested for various characteristics and performances:
[0127] (1) Observe the appearance of the template glue and test the viscosity.
[0128] (2) The template glue is evenly introduced into the dumbbell mold, ensuring that there are no bubbles in the glue liquid, and the glue surface is kept level with the mold surface. The glue is completely cured by UV light to obtain a rubber strip. The tensile strength, elongation at break, and Young's modulus of the rubber strip are tested.
[0129] (3) The template glue is evenly introduced into a mold with a diameter of Φ40 mm and a thickness of 5 mm, ensuring that there are no bubbles in the glue liquid and that the glue surface is kept level with the mold surface. The glue is completely cured with UV light to obtain a glue block, and the hardness of the resulting glue strip is tested after curing.
[0130] (4) Use a hydrometer to measure the liquid density before the glue is cured, use a densitometer to measure the density of the cured glue block, and calculate the volume shrinkage rate before and after the glue is cured.
[0131] (5) The glue is evenly spin-coated on a glass wafer with a thickness of 1 μm, and is completely cured by UV light to obtain a film. The surface water drop angle of the newly prepared template glue is detected.
[0132] (6) The prepared template glue was used to replicate the working mold on the hard template, and then the finished nanoimprint glue was imprinted on the glass wafer for 15 consecutive times. The structural integrity was observed macroscopically, and the microstructure was observed by SEM to see if there were any defects or size differences.
[0133] The test results are shown in Table 4:
[0134] Table 4: Performance test results
[0135]
[0136] It can be seen from the test results in Table 4 that the template glue obtained by the present invention has an appearance of a colorless to light yellow transparent liquid, a viscosity of 400-500 mPa.s, and good fluidity; after curing, the hardness reaches below 90A, the tensile strength reaches above 6.5 MPa, and the Young's modulus reaches above 50 MPa, showing excellent toughness and mechanical strength; the volume shrinkage rate after curing is below 3%, showing ultra-low shrinkage; the surface water drop angle of the newly made template reaches above 115°, the surface energy is low, and continuous imprinting is repeated for multiple times, and the demolding can be complete, thereby improving the demolding efficiency.
[0137] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.
Claims
1. A nanoimprint template glue, characterized in that: It is prepared from raw materials comprising the following components in mass ratio: Epoxy modified polysiloxane resin 10%~25%; Organic silicon fluorine modified polyurethane acrylic resin 20%~30%; Fluorine-modified acrylate 15%~25%; Modified epoxy acrylic resin 5%~10%; Cationic hybrid acrylic resin 12%~25%; Cross-linking diluent 3%~5%; Flexible chain extender 1%~3%; Photoinitiator 1%~3%; Cationic initiator 1%~2%; The epoxy-modified polysiloxane resin is prepared by the following preparation method: silicone oil and 4-vinyl cyclohexyl oxide are mixed and reacted to obtain epoxy-modified polysiloxane resin; the hydrogen content of the silicone oil is 1.5wt% to 1.65wt%; The organic silicon fluorine-modified polyurethane acrylic resin is at least one of UV-9843A, UV-9843-1, UV-9843-2, Trust-7760, FSP8658, and LuCure8696; The fluorine-modified acrylate is at least one of perfluorooctyl ethyl acrylate, dodecafluoroheptyl methacrylate, (N-methylperfluorohexylsulfonamido)ethyl acrylate, perfluorohexyl ethyl acrylate, perfluorohexyl ethyl methacrylate, perfluorobutyl ethyl acrylate and 1H,1H,2H,2H-perfluorooctanol acrylate; The modified epoxy acrylic resin is at least one of Ebecryl600, Agisyn 6050TF, WORLD ROCK 700, 3,4-epoxycyclohexyl methyl methacrylate and neopentyl glycol polymethyl ethylene oxide diacrylate; The cationic hybrid acrylic resin is a cationic hybrid UV resin and is at least one of U-9100A, U-9100B, U-9101, U-9103, U-9200, U-9210, U-9310 and U-9340.
2. The nanoimprint template glue according to claim 1, characterized in that: The mass ratio of the silicone oil to 4-vinyl epoxyhexane is 27.5 to (29.5 to 31); The reaction is carried out under the action of a catalyst; the catalyst is a rhodium catalyst; the mass ratio of the catalyst to the silicone oil is (0.095-0.1):
100.
3. The nanoimprint template glue according to claim 1 or 2, characterized in that: The preparation method specifically comprises: The silicone oil, 4-vinyl cyclohexene oxide and the catalyst are mixed, stirred at 30-40° C. for 24-36 hours, and then heated to 80-90° C. and stirred for 3-5 hours to obtain an epoxy-modified polysiloxane resin.
4. The nanoimprint template glue according to claim 1, characterized in that: The cross-linking diluent is at least one of hydroxybutyl vinyl ether, triethylene glycol divinyl ether, 1,4-cyclohexyl dimethanol divinyl ether, butyl vinyl ether, 1,6-hexanediol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, tris(2-hydroxyethyl)isocyanuric acid triacrylate, di(trimethylolpropane) tetraacrylate, 4(ethoxylated) pentaerythritol tetraacrylate and pentaerythritol tetraacrylate; The flexible chain extender is at least one of 3 (ethoxy) trimethylolpropane triacrylate, 6 (ethoxy) trimethylolpropane triacrylate, 9 (ethoxy) trimethylolpropane triacrylate, 15 (ethoxy) trimethylolpropane triacrylate, and 20 (ethoxy) trimethylolpropane triacrylate; The photoinitiator is at least one of photoinitiator 1173, photoinitiator 184, IPO, photoinitiator 127, photoinitiator 369, photoinitiator ITX, photoinitiator BDK and photoinitiator 819; The cationic initiator is ANTHRACURE ™ UVS-1331、ANTHRACURE ™ At least one of UVS-1101, Easepi 6992, Easepi 1176 and Easepi 250.
5. A method for preparing a nanoimprint template glue according to any one of claims 1 to 4, characterized in that: The following steps are involved: a) mixing an organosilicon fluorine-modified polyurethane acrylic resin, a modified epoxy acrylic resin, a fluorine-modified acrylate, a cross-linking diluent and a flexible chain extender to obtain a mixed solution 1; b) mixing the mixed solution 1 with a photoinitiator, a cationic initiator and a cationic hybrid acrylic resin to obtain a mixed solution 2; c) mixing the mixed solution 2 with an epoxy-modified polysiloxane resin to obtain a mixed solution 3; d) Degassing and sieve filtering the mixed solution 3 to obtain a nanoimprint template glue.
6. The preparation method according to claim 5, characterized in that: The specific steps include: a) Add organic silicon fluorine-modified polyurethane acrylic resin, modified epoxy acrylic resin, fluorine-modified acrylate, cross-linking diluent and flexible chain extender into a container, stir at a rate of 600-800 r / min for 20-30 min, and then stir at a rate of 1000-1200 r / min for 20-30 min to obtain a mixed solution 1; during the above process, the liquid temperature in the container is maintained at 10±1°C; b) adding a photoinitiator, a cationic initiator and a cationic hybrid acrylic resin into the container, stirring at a rate of 1000-1200 r / min for 30-40 min to obtain a mixed solution 2; during the above process, the liquid temperature in the container is maintained at 10±1° C.; c) adding epoxy-modified polysiloxane resin into the container, stirring at a rate of 1000-1200 r / min for 30-40 min to obtain a mixed solution 3; d) Degassing and sieve filtering the mixed solution 3 to obtain a nanoimprint template glue.
Citation Information
Patent Citations
Ultraviolet-heat dual curing optical adhesive containing epoxidized polybutadiene resin
CN104449419A
Track plate surface coating with good weather fastness
CN105670397A