A corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy film material and its preparation process

Through the magnetron sputtering preparation of FeCoNiCuAl high-entropy alloy film material, the problem of difficult high-entropy alloy films to have both magnetism and corrosion resistance is solved, and high-performance corrosion resistance and magnetism are achieved, which is suitable for electronic information in harsh environments. Device.

CN116043139BActive Publication Date: 2024-11-22SHANGHAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310127009.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-16
Publication Date
2024-11-22
Estimated Expiration
2043-02-16

AI Technical Summary

Technical Problem

Existing high-entropy alloy films are difficult to have both magnetic properties and corrosion resistance, and usually reduce magnetic properties in order to improve corrosion resistance.

Method used

FeCoNiCuAl high-entropy alloy thin film material is prepared by magnetron sputtering technology, and appropriate process parameters are selected to ensure uniform distribution of elements, form an amorphous structure, avoid Cr elements to improve corrosion resistance, and maintain good magnetism.

Benefits of technology

It realizes the corrosion resistance and magnetism of high-entropy alloy films, has low corrosion current density, and shows soft magnetic properties. It is suitable for the field of electronic information devices, and has a simple preparation process and is cost-saving.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116043139B_ABST
    Figure CN116043139B_ABST
Patent Text Reader

Abstract

The present invention relates to a corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy thin film material and a preparation process thereof, and belongs to the field of multi-principal alloy thin film materials. The main components of the thin film material include the following atomic percentage compositions: Fe: 15.0-25.0%, Co: 15.0-25.0%, Ni: 15.0-25.0%, Cu: 15.0-25.0%, Al: 15.0-25.0%. The preparation steps include ultrasonic cleaning of the substrate, vacuum chamber evacuation and filling with argon, pre-sputtering and sputtering. Compared with the prior art, the surface of the film prepared by the present invention is smooth and flat, the structure is in a disordered state, and it has both magnetic properties and corrosion resistance. The preparation method of the present invention has strong feasibility, high repeatability, and is easy to apply and promote.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of multi-principal alloy thin film materials, and in particular to a novel corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy thin film material and a preparation process thereof. Background Art

[0002] The history of thin film can be traced back to more than 3,000 years ago, when ancient China began to use glaze coatings in ceramics. In the early 19th century, it was discovered that the glow discharge process could deposit solid thin films. After the 20th century, thin film preparation methods such as electrolysis, chemical reaction and vacuum evaporation came out one after another, and thin film technology developed rapidly. Among them, optical thin films were the first to be studied and applied. Various optical thin films such as anti-reflection films, high-reflection films, filter films, and spectroscopic films were successfully prepared and widely used in optical instruments, solar cells, architectural glass and other fields. After the 1950s, the advancement of microelectronics technology has greatly promoted the advancement of thin film technology. In the modern integrated circuit manufacturing process, thin film deposition and etching are essential thin film processes.

[0003] In terms of function and application, thin films can be divided into: electrical thin films, used for resistors, semiconductors, etc.; optical thin films, used for reflection, anti-reflection, spectroscopy, etc.; acoustic thin films, used for acoustic transmission, piezoelectricity, etc.; magnetic thin films, used for information recording, storage, disks, magnetic heads, etc. Especially for magnetic devices that occupy a large volume and weight in modern electronic devices, such as inductors and transformers, their miniaturization, lightness, multi-function and high frequency have become a trend and are increasingly attracting the attention of researchers.

[0004] In recent years, a new alloy system, high entropy alloy, has been proposed. It breaks the design concept of traditional alloys. It is no longer based on one or two metals, but consists of five or more elements in equimolar or nearly equimolar proportions. The atomic percentage of each element is between 5% and 35%. It has four inherent effects: high entropy effect, lattice distortion effect, hysteresis diffusion effect, and "cocktail" effect, which give it good comprehensive performance and will be potentially used in many fields. Patent CN202210305011.5 discloses a TiAlMoNbW high entropy alloy target and its preparation process. The high entropy alloy target component includes Ti, Al, Mo, Nb, and W. The atomic ratio of its constituent elements is Ti:Al:Mo:Nb:W=1:1:1:1:1at.%, the target grain size is 1-20μm, and the density of the target is more than 98%. This type of high entropy alloy target has high uniformity and high density, and can be used to prepare highly wear-resistant and corrosion-resistant films, but it cannot have both magnetism and corrosion resistance at the same time.

[0005] High entropy films, like high entropy alloys, also have excellent properties and a wider range of applications. With the booming semiconductor industry, the demand for films that have both magnetic and corrosion resistance is particularly urgent. High entropy alloys often contain ferromagnetic elements such as Fe, Co, and Ni, which give them excellent magnetic properties. However, at present, in order to obtain excellent corrosion resistance, the prepared films often contain a high content of antiferromagnetic element Cr, which will greatly reduce the magnetic properties of the film.

[0006] Therefore, a FeCoNiCuAl film having both magnetic properties and corrosion resistance and a preparation process thereof are needed. Summary of the invention

[0007] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy thin film material, which solves the problem that the magnetic film has poor corrosion resistance and cannot serve for a long time.

[0008] In order to achieve the above object, the present invention adopts the following inventive concept:

[0009] Common bulk high entropy alloys often have high contents of Fe, Co, and Ni ferromagnetic elements, which give high entropy alloys excellent magnetic properties. In addition, the four major effects unique to high entropy alloys often give them excellent comprehensive performance. However, due to the limitations of the preparation method, bulk high entropy alloys often have component segregation, which will have unpredictable effects on the performance of the material. According to the characteristics of magnetron sputtering, the present invention has found through a large number of experimental studies that after selecting appropriate process parameters, all elements of the prepared thin film material are evenly distributed, and the expected performance requirements can be achieved: both corrosion resistance and magnetism. The thin film material prepared by the present invention is an amorphous structure. According to the present invention, the FeCoNiCuAl high entropy alloy thin film material has the advantages of good magnetism, corrosion resistance, simple preparation process and wide application.

[0010] According to the above inventive concept, the present invention adopts the following technical solution:

[0011] A corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy film material, the main components of which include the following atomic percentage compositions: Fe: 15.0-25.0%, Co: 15.0-25.0%, Ni: 15.0-25.0%, Cu: 15.0-25.0%, Al: 15.0-25.0%.

[0012] Furthermore, the structure of the film material is amorphous, and the corrosion current density is 1.41×10 -6 A / cm 2 .

[0013] Preferably, the atomic ratio of the constituent elements in the thin film material is Fe:Co:Ni:Cu:Al=1:1:1:0.8:0.8.

[0014] Furthermore, the thickness of the thin film material is 300-600 nm.

[0015] The method for preparing the above-mentioned corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy thin film material comprises the following steps:

[0016] (1) Preparing a target material: selecting a FeCoNiCuAl high entropy alloy target material containing five elements: Fe, Co, Ni, Cu, and Al;

[0017] (2) Prepare the substrate: single-sided polishing <100> Si was cut into required sizes, ultrasonically cleaned in acetone, alcohol, and deionized water in sequence, and blown dry from the side and placed on the sample stage of the magnetron sputtering vacuum chamber;

[0018] (3) Sputtering deposition of thin films

[0019] 3a) Pre-evacuate to 2-5 Pa, and continue to evacuate to 3×10 -4 Pa~6×10 -4 Pa, argon is introduced as the working gas;

[0020] 3b) pre-sputtering the target material to remove oxides and contaminants on the surface of the high entropy alloy target material;

[0021] 3c) performing sputtering: DC magnetron sputtering, with a power of 55-75 W, a substrate rotation speed of 15-25 rpm / min, and a sputtering time controlled at 50-70 min. After the sputtering, a sample with a high entropy alloy film deposited thereon is obtained.

[0022] Furthermore, the obtained sample can be further subjected to vacuum annealing treatment to further improve its performance.

[0023] The distance between the substrate and the target is 8 to 10 cm.

[0024] The working gas in step 3a) is argon with a purity of 99.999%.

[0025] The pre-sputtering power of step 3b) is controlled at 75-100 W, the sputtering gas pressure is controlled at 0.60-0.80 Pa, and the pre-sputtering time is 5-10 min.

[0026] The sputtering gas pressure in step 3c) is 0.50-0.70 Pa.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1. Compared with traditional bulk high entropy alloys, the alloy elements selected in the present invention do not contain Cr, but only contain five elements, FeCoNiCuAl, and can also achieve the high entropy effect, lattice distortion effect, hysteresis diffusion effect, "cocktail" effect and other effects of the existing six or more elements such as FeCoNiCrCuAlMn and FeCoNiCrCuAl, and obtain a film with high corrosion resistance and good magnetic properties. Fe, Co, and Ni are ferromagnetic elements, and most high entropy alloys contain these three elements. Cr is an antiferromagnetic element, which will greatly reduce the magnetic properties of the material. The alloy film system of the present invention, on the basis of not containing Cr, adopts Cu and Al elements with good corrosion resistance, and greatly improves the corrosion resistance on the basis of ensuring certain magnetic properties or slightly sacrificing magnetic properties.

[0029] 2. The present invention adopts the method of DC magnetron sputtering, and selects single-sided polishing <100> Si is used as the substrate. DC magnetron sputtering has a higher efficiency in film preparation. The ionized atoms move in a cycloidal motion on the target surface due to the magnetic field, and the target atoms can be sputtered out more quickly. Compared with traditional DC sputtering, it can also improve the utilization rate of the target on the basis of being faster. Si is the most commonly used semiconductor material with stable structure and performance. When used as a sputtering substrate, it can make the sputtered atoms more closely combined, and it is convenient for repeated experiments and subsequent performance testing. The surface of the prepared high-entropy alloy film is smooth, with an amorphous structure, and all elements are evenly distributed. It has excellent corrosion resistance, and the corrosion current density is 1.41×10 -6 A / cm 2 , and exhibits soft magnetic properties, and is expected to be used as a thin film sensor in the field of electronic information devices in harsh environments.

[0030] 3. The high entropy alloy film prepared by the present invention has a convenient preparation process and saves costs. It can be plated on the surface of common steel to achieve the effect of improving surface performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a scanning electron microscope image of the FeCoNiCuAl thin film material of Example 1 of the present invention;

[0032] Figure 2 This is the XRD spectrum of the FeCoNiCuAl thin film material of Example 1 of the present invention;

[0033] Figure 3 This is a scanning electron microscope image of the FeCoNiCuAl thin film material after annealing at 673K ​​according to Example 2 of the present invention;

[0034] Figure 4 The XRD spectrum of the FeCoNiCuAl thin film material after annealing at 673K ​​according to Example 2 of the present invention;

[0035] Figure 5 This is a scanning electron microscope image of the FeCoNiCuAl thin film material after annealing at 873K according to Example 3 of the present invention;

[0036] Figure 6 This is the XRD spectrum of the FeCoNiCuAl thin film material after annealing at 873K in Example 3 of the present invention. DETAILED DESCRIPTION

[0037] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings. The following embodiments or drawings are used to illustrate the present invention but are not used to limit the scope of the present invention.

[0038] If the specific conditions are not specified in the examples, the conventional conditions or the conditions recommended by the manufacturer are used. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. For example, the method used in the present invention can use commercially available magnetron sputtering coating equipment.

[0039] Embodiment 1:

[0040] A new type of corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy film material, the main components of which are composed of the following atomic percentages: Fe: 21%, Co: 21%, Ni: 21%, Cu: 18%, Al: 19%.

[0041] In this embodiment, a method for preparing a novel corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy thin film material comprises the following steps:

[0042] (1) preparing a target material: selecting a FeCoNiCuAl high entropy alloy target material containing five elements of Fe, Co, Ni, Cu, and Al, wherein the atomic ratio of the constituent elements is 1:1:1:0.8:0.8;

[0043] (2) Prepare the substrate: single-sided polishing <100> Si was cut into required sizes, ultrasonically cleaned in acetone, alcohol, and deionized water in turn, blown dry from the side, and placed on the sample stage of the magnetron sputtering vacuum chamber; the distance between the substrate and the target was 9 cm;

[0044] (3) Sputtering deposition of thin films

[0045] 3a. Pre-vacuum to 5Pa, and continue to vacuum to 5×10 -4 Pa, argon gas with a purity of 99.999% is introduced as the working gas;

[0046] 3b. Pre-sputter the target to remove oxides and contaminants on the surface of the high entropy alloy target. The pre-sputtering power is controlled at 80 W, the sputtering pressure is controlled at 0.70 Pa, and the pre-sputtering time is 8 min.

[0047] 3c. Sputtering: DC magnetron sputtering, power of 60 W, sputtering gas pressure of 0.6 Pa, substrate rotation speed of 18 rpm / min, sputtering time controlled at 60 min, after the sputtering is completed, a sample with a high entropy alloy film deposited is obtained.

[0048] Experimental test analysis

[0049] See also Figure 1 The scanning electron microscopy results show that the surface of the prepared high entropy film is smooth and has no obvious defects. The XRD diffraction pattern ( Figure 2 ) shows that the film is an amorphous structure. The magnetic properties were tested using a vibrating sample magnetometer at room temperature with an applied magnetic field of 3.98×10 5 A / m, and the coercive force is 2kA / m; the polarization curve is tested using an electrochemical workstation and the corrosion current density is 1.4×10 -6 A / cm 2 , which is better than the commonly used 304 stainless steel. This shows that the film has obvious soft magnetic properties and excellent corrosion resistance.

[0050] Embodiment 2:

[0051] This embodiment is basically the same as Embodiment 1, except that:

[0052] In this embodiment, the prepared film is kept at 673K ​​for 1 hour in a vacuum annealing furnace. The details are as follows:

[0053] In this embodiment, a method for preparing a novel corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy thin film material comprises the following steps:

[0054] (1) preparing a target material: selecting a FeCoNiCuAl high entropy alloy target material containing five elements of Fe, Co, Ni, Cu, and Al, wherein the atomic ratio of the constituent elements is 1:1:1:0.8:0.8;

[0055] (2) Prepare the substrate: single-sided polishing <100> Si was cut into required sizes, ultrasonically cleaned in acetone, alcohol, and deionized water in turn, blown dry from the side, and placed on the sample stage of the magnetron sputtering vacuum chamber; the distance between the substrate and the target was 9 cm;

[0056] (3) Sputtering deposition of thin films;

[0057] 3a. Pre-vacuum to 5Pa, and continue to vacuum to 5×10 -4 Pa, argon is introduced as the working gas;

[0058] 3b. Pre-sputter the target material to remove oxides and contaminants on the surface of the high entropy alloy target material; the pre-sputtering power is controlled at 80W, the sputtering pressure is controlled at 0.70Pa, and the pre-sputtering time is 8min;

[0059] 3c. Sputtering: DC magnetron sputtering, power of 60 W, sputtering gas pressure of 0.6 Pa, substrate rotation speed of 18 rpm / min, sputtering time controlled at 60 min, after the sputtering is completed, a sample with a high entropy alloy film deposited is obtained.

[0060] (4) Perform vacuum annealing treatment.

[0061] 4a. Place the sample in a quartz glass tube and evacuate it to 5 Pa first, then evacuate it to 5×10 -4 Pa;

[0062] 4b. Raise the temperature of the furnace chamber to 673K, push the quartz glass tube containing the sample into the chamber, and keep it warm for 1 hour;

[0063] 4c. When the holding time is over, turn off the heating system, cool to room temperature with the furnace, and take out the sample.

[0064] Experimental test analysis

[0065] This embodiment adopts vacuum annealing process, and the surface of the film after annealing is relatively flat ( Figure 3 ), XRD pattern ( Figure 4 ) shows that it is still an amorphous structure. The sample and substrate of this embodiment were subjected to electrochemical experiments in NaCl corrosive medium, and the corrosion current density was 2.7×10 -7 A / cm 2 , the corrosion resistance has been improved. The magnetic properties were tested using a vibrating sample magnetometer at room temperature with an applied magnetic field of 3.98×10 5 A / m, coercive force 4.2kA / m, still showing soft magnetic properties.

[0066] Embodiment 3:

[0067] This embodiment is basically the same as the first embodiment, except that:

[0068] In this embodiment, the prepared film is kept at 873K for 1 hour in a vacuum annealing furnace; the details are as follows:

[0069] In this embodiment, a method for preparing a novel corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy thin film material comprises the following steps:

[0070] (1) preparing a target material: selecting a FeCoNiCuAl high entropy alloy target material containing five elements of Fe, Co, Ni, Cu, and Al, wherein the atomic ratio of the constituent elements is 1:1:1:0.8:0.8;

[0071] (2) Prepare the substrate: single-sided polishing <100> Si was cut into required sizes, ultrasonically cleaned in acetone, alcohol, and deionized water in sequence, and blown dry from the side and placed on the sample stage of the magnetron sputtering vacuum chamber;

[0072] (3) Sputtering deposition of thin films

[0073] 3a. Pre-vacuum to 5Pa, and continue to vacuum to 5×10 -4 Pa, argon is introduced as the working gas;

[0074] 3b. Pre-sputter the target material to remove oxides and contaminants on the surface of the high entropy alloy target material; the pre-sputtering power is controlled at 80W, the sputtering pressure is controlled at 0.70Pa, and the pre-sputtering time is 8min;

[0075] 3c. Sputtering: DC magnetron sputtering, power of 60 W, sputtering gas pressure of 0.6 Pa, substrate rotation speed of 18 rpm / min, sputtering time controlled at 60 min, after the sputtering is completed, a sample with a high entropy alloy film deposited is obtained.

[0076] (4) Vacuum annealing

[0077] 4a. Place the sample in a quartz glass tube and evacuate it to 5 Pa first, then evacuate it to 5×10 -4 Pa;

[0078] 4b. Raise the temperature of the furnace chamber to 873K, push the quartz glass tube containing the sample into the chamber, and keep it warm for 1 hour;

[0079] 4c. When the holding time is over, turn off the heating system, cool to room temperature with the furnace, and take out the sample.

[0080] Experimental test analysis

[0081] This embodiment adopts vacuum annealing process, and a large number of small precipitates appear on the surface of the film after annealing ( Figure 5 ), XRD pattern ( Figure 6 ) shows that there are more crystallized phases, which may be a single FCC phase. The sample and substrate of this example were subjected to electrochemical experiments in NaCl corrosion medium, and the corrosion current density was 5.23×10 -7 A / cm 2 , the corrosion resistance of the film is still improved compared with the original state; the magnetic properties of the film were tested using a vibrating sample magnetometer at room temperature and an external magnetic field of 3.98×10 5A / m, the coercive force is 21kA / m, and the soft magnetic properties are slightly reduced, but it still has the magnetic properties required for sensors.

[0082] In summary, the corrosion-resistant magnetic FeCoNiCuAl thin film material of the above embodiment has the following main components in atomic percentage: Fe: 15.0-25.0%, Co: 15.0-25.0%, Ni: 15.0-25.0%, Cu: 15.0-25.0%, Al: 15.0-25.0%. After being prepared by magnetron sputtering with appropriate parameters and annealing treatment, a high entropy alloy film with both corrosion resistance and magnetism is obtained. The FeCoNiCuAl high entropy thin film material of the above embodiment of the present invention has the advantages of both magnetic properties and corrosion resistance and simple preparation process.

[0083] Example 4

[0084] A method for preparing a novel corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy thin film material comprises the following steps:

[0085] (1) Target preparation: A FeCoNiCuAl high entropy alloy target containing five elements of Fe, Co, Ni, Cu, and Al is selected, and the atomic ratio of the constituent elements is 1:1:1:0.8:0.8; the distance between the substrate and the target is 8 cm;

[0086] (2) Prepare the substrate: single-sided polishing <100> Si was cut into required sizes, ultrasonically cleaned in acetone, alcohol, and deionized water in sequence, and blown dry from the side and placed on the sample stage of the magnetron sputtering vacuum chamber;

[0087] (3) Sputtering deposition of thin films

[0088] 3a. Pre-vacuum to 2Pa, and continue to vacuum to 3×10 -4 Pa, argon gas with a purity of 99.999% is introduced as the working gas;

[0089] 3b. Pre-sputter the target material to remove oxides and contaminants on the surface of the high entropy alloy target material; the pre-sputtering power is controlled at 75W, the sputtering pressure is controlled at 0.60Pa, and the pre-sputtering time is 5min;

[0090] 3c. Sputtering: DC magnetron sputtering, power of 55 W, sputtering gas pressure of 0.50 Pa; substrate rotation speed of 15 rpm / min, sputtering time controlled at 50 min, after the sputtering is completed, a sample with a high entropy alloy film deposited is obtained.

[0091] The magnetic and corrosion resistance tests of the obtained samples are as follows:

[0092] The magnetic properties were tested using a vibrating sample magnetometer at room temperature with an applied magnetic field of 3.98×10 5 A / m, and the coercive force is 1.8kA / m; the polarization curve is tested using an electrochemical workstation and the corrosion current density is 2.5×10 -6 A / cm 2 , which is comparable to the corrosion resistance of commonly used 304 stainless steel.

[0093] Example 5

[0094] A method for preparing a novel corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy thin film material comprises the following steps:

[0095] (1) Target preparation: A FeCoNiCuAl high entropy alloy target containing five elements of Fe, Co, Ni, Cu, and Al is selected, and the atomic ratio of the constituent elements is 1:1:1:0.8:0.8; the distance between the substrate and the target is 10 cm;

[0096] (2) Prepare the substrate: single-sided polishing <100> Si was cut into required sizes, ultrasonically cleaned in acetone, alcohol, and deionized water in sequence, and blown dry from the side and placed on the sample stage of the magnetron sputtering vacuum chamber;

[0097] (3) Sputtering deposition of thin films

[0098] 3a. Pre-vacuum to 5Pa, and continue to vacuum to 6×10 -4 Pa, argon gas with a purity of 99.999% is introduced as the working gas;

[0099] 3b. Pre-sputter the target to remove oxides and contaminants on the surface of the high entropy alloy target; the pre-sputtering power is controlled at 100 W, the sputtering pressure is controlled at 0.80 Pa, and the pre-sputtering time is 10 min;

[0100] 3c. Sputtering: DC magnetron sputtering, power of 75 W, sputtering gas pressure of 0.70 Pa; substrate rotation speed of 25 rpm / min, sputtering time controlled at 70 min, after the sputtering is completed, a sample with a high entropy alloy film deposited is obtained.

[0101] The magnetic and corrosion resistance tests of the obtained samples are as follows:

[0102] The magnetic properties were tested using a vibrating sample magnetometer at room temperature with an applied magnetic field of 3.98×10 5 A / m, and the coercive force is 3.2kA / m; the polarization curve is tested using an electrochemical workstation and the corrosion current density is 3.6×10 -6 A / cm 2 , which is comparable to the corrosion resistance of commonly used 304 stainless steel.

[0103] The above describes the embodiments of the present invention in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made according to the purpose of the invention. Any changes, modifications, substitutions, combinations or simplifications made according to the spirit and principle of the technical solution of the present invention should be equivalent replacement methods. As long as they meet the purpose of the invention, they belong to the protection scope of the present invention.

Claims

1. A corrosion-resistant magnetic FeCoNiCuAl high entropy alloy thin film material, characterized in that: Its composition is composed of the following atomic percentages: Fe: 15.0-25.0%, Co: 15.0-25.0%, Ni: 15.0-25.0%, Cu: 15.0-25.0%, Al: 15.0-25.0%; the thickness of the film material is 300-600nm; the organizational structure of the film material is amorphous; The film material is prepared by the following method: (1) Prepare the target material: select FeCoNiCuAl high entropy alloy target containing five elements: Fe, Co, Ni, Cu and Al; (2) Prepare the substrate: single-sided polishing <100> Si is cut into required sizes, cleaned and dried, and then placed on the sample stage of the magnetron sputtering vacuum chamber; (3) Sputtering deposition of thin films 3a) Pre-evacuate to 2~5 Pa, and continue to evacuate to 3×10 -4 Pa~6×10 -4 Pa, argon is introduced as the working gas; 3b) Pre-sputtering the target to remove oxides and contaminants on the surface of the high entropy alloy target; 3c) performing sputtering: DC magnetron sputtering, with a power of 55-75 W, a substrate rotation speed of 15-25 rpm / min, and a sputtering time controlled at 50-70 min. After the sputtering, a sample with a high entropy alloy film deposited thereon is obtained; The atomic ratio of the constituent elements in the thin film material is Fe:Co:Ni:Cu:Al=1:1:1:0.8:0.

8.

2. A corrosion-resistant magnetic FeCoNiCuAl high entropy alloy thin film material according to claim 1, characterized in that: The corrosion current density of the film material is 1.41×10 -6 A / cm 2 .

3. A method for preparing the corrosion-resistant magnetic FeCoNiCuAl high entropy alloy thin film material as claimed in any one of claims 1 to 2, characterized in that: The steps include: (1) Prepare the target material: select FeCoNiCuAl high entropy alloy target containing five elements: Fe, Co, Ni, Cu and Al; (2) Prepare the substrate: single-sided polishing <100> Si is cut into required sizes, cleaned and dried, and then placed on the sample stage of the magnetron sputtering vacuum chamber; (3) Sputtering deposition of thin films 3a) Pre-evacuate to 2~5 Pa, and continue to evacuate to 3×10 -4 Pa~6×10 -4 Pa, argon is introduced as the working gas; 3b) Pre-sputtering the target to remove oxides and contaminants on the surface of the high entropy alloy target; 3c) Sputtering: DC magnetron sputtering, the power is 55~75 W, the substrate rotation speed is 15~25 rpm / min, the sputtering time is controlled at 50~70 min, and a sample with a high entropy alloy film deposited is obtained after the sputtering is completed.

4. The method for preparing a corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy thin film material according to claim 3, characterized in that: In step (2), the cleaning is performed by ultrasonic cleaning in acetone, alcohol, and deionized water in sequence, and the drying is performed from the side.

5. The method for preparing a corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy thin film material according to claim 3, characterized in that: The distance between the substrate and the target is 8~10cm.

6. The method for preparing a corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy thin film material according to claim 3, characterized in that: The working gas in step 3a) is argon with a purity of 99.999%.

7. The method for preparing a corrosion-resistant magnetic FeCoNiCuAl high-entropy alloy thin film material according to claim 3, characterized in that: In step 3b), the pre-sputtering power is controlled at 75-100 W, the sputtering pressure is controlled at 0.60-0.80 Pa, and the pre-sputtering time is 5-10 min.