A cerium-supported silver-supported catalytic adsorbent for flue gas demercuration and denitrification, and its preparation method and application
By loading CeO2 and silver nanoparticles on EVS-10 molecular sieve, the cerium-loaded silver catalytic adsorbent solves the problem of synergistic removal of mercury and nitrogen oxides in coal-fired flue gas, achieving efficient and stable removal effects. And the catalyst's resistance to sulfur poisoning and recycling ability are improved.
Patent Information
- Application Number
- CN202111276250.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-10-29
AI Technical Summary
It is difficult to efficiently remove mercury and nitrogen oxides from coal-fired power plant flue gas at the same time with existing technology, and existing catalysts are prone to agglomeration when repeatedly recycled, affecting denitrification performance.
Using cerium-loaded silver catalytic adsorbent, by first loading CeO2 active component on EVS-10 molecular sieve, and then loading silver nanoparticles, synergistic removal of mercury and nitrogen oxides is achieved, and the catalyst's performance is improved through a specific preparation method. Stability and recyclability.
It achieves efficient synergistic removal of mercury and nitrogen oxides. The catalyst shows good resistance to SO2 poisoning and long service life in complex flue gas environments, reducing overall costs and is suitable for industrial production and equipment upgrading.
Smart Images

Figure BDA0003330026640000121 
Figure BDA0003330026640000122 
Figure BDA0003330026640000131
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of environmental protection and air pollution control, and in particular to a cerium-supported silver-supported catalytic adsorbent for flue gas demercurization and denitrification, and a preparation method and application thereof. Background Art
[0002] Mercury is a toxic heavy metal that causes serious harm to human health and the ecological environment. Coal-fired power plants are considered to be the world's largest source of anthropogenic mercury emissions. Therefore, it is imperative to study the technology of efficiently removing mercury from the flue gas of coal-fired power plants. Coal-fired power plants are considered to be one of the most important sources of anthropogenic mercury emissions. Mercury in flue gas is mainly in the form of Hg 2+ , Hg p and Hg 0 There are three forms, Hg 2+ It is soluble in water and can therefore be removed efficiently by the pollutant control equipment wet flue gas desulfurization device; Hg p Since it is combined with fly ash, it can be removed by particulate matter control equipment such as bag filters or electrostatic precipitators; however, Hg 0 It is insoluble in water and volatile, and is quite stable at low temperatures. It is difficult to be removed by the existing pollutant control equipment in power plants and is directly discharged into the atmosphere. Therefore, the key to removing mercury from flue gas in coal-fired power plants is to control Hg 0 emissions.
[0003] At present, the two main research directions of mercury removal are adsorbent demercuration and catalytic oxidation demercuration: Adsorbent demercuration is to remove Hg 0 Through physical or chemical adsorption to the adsorbent surface, and then removed by the particulate matter control equipment; catalytic oxidation demercuration is to remove Hg 0 Highly efficient oxidation to Hg 2+ , and then removed by the wet desulfurization device. In our previous research, we synthesized a new type of catalytic adsorption material - EVS-10 molecular sieve silver-loaded material. EVS-10 is a type of molecular sieve in which vanadium completely replaces titanium in the titanium silicate molecular sieve ETS-10. It is mainly composed of vanadium oxygen octahedrons and silicon oxygen tetrahedrons, and is linked by common corner oxygen atoms to finally form a three-dimensional network structure. Since the EVS-10 molecular sieve framework contains vanadium active components, it has a certain catalytic ability, similar to industrial vanadium-loaded catalysts, and can catalytically oxidize elemental mercury. The experimental test results show that the efficiency of EVS-10 molecular sieve catalytic oxidation of mercury is about 48%. Silver nanoparticles can adsorb elemental mercury to form a stable alloy, namely amalgam. Amalgam is a relatively strong interaction, stronger than the intermolecular force, so the silver-loaded adsorbent is a type of adsorbent with extremely high mercury removal efficiency and capacity. The comprehensive mercury removal efficiency of EVS-10 molecular sieve silver-loaded material reaches 100%. Although the material has good mercury removal performance, it has a single function and can only be used for the control of single pollutant mercury, and the denitrification performance is poor.
[0004] In addition to elemental mercury, nitrogen oxides are also a common air pollutant produced by coal combustion, which can cause acid rain and greenhouse effect. The proportion of NO in nitrogen oxides (NOx) accounts for more than 95%, so the key to removing nitrogen oxides is to remove NO. At present, the most effective and widely used technology for removing NO from coal-fired flue gas is NH3 selective catalytic reduction (SCR) technology. The SCR catalysts currently studied are mainly prepared by loading metal oxides such as V2O5, CuO, Cr2O3, CeO2, Fe2O3, MnO2, Co2O3, etc. on carriers such as Al2O3, SiO2, TiO2, ZrO2, carbon materials and molecular sieves. Although EVS-10 molecular sieve has a certain ability to remove mercury as a catalyst carrier, its catalytic denitrification performance is poor (only 14% removal efficiency), and it cannot achieve the purpose of simultaneous mercury removal and denitrification; and it is easy to agglomerate into larger particles during repeated recycling, which is not conducive to the repeated recycling of molecular sieves. Summary of the invention
[0005] The purpose of the present disclosure is to provide a cerium-supported silver-supported catalytic adsorbent for flue gas demercuration and denitrification, and a preparation method and application thereof, wherein the catalytic adsorbent can achieve the synergistic removal of mercury and nitrogen oxides and can be easily recycled and reused.
[0006] In order to achieve the above-mentioned objectives, the first aspect of the present disclosure provides a cerium-loaded silver-loaded catalytic adsorbent for flue gas demercurization and denitrification, the catalytic adsorbent comprising a carrier and silver nanoparticles and an active component loaded on the carrier; wherein the carrier comprises an EVS-10 molecular sieve, and the active component comprises CeO2, wherein the active component is first loaded on the EVS-10 molecular sieve, and the silver nanoparticles are subsequently loaded on the EVS-10 molecular sieve.
[0007] Optionally, based on the total weight of the catalytic adsorbent, the mass fraction of the carrier is 45-98 weight %, the mass fraction of the silver nanoparticles is 1-40 weight %, and the mass fraction of the active component is 1-15 weight %.
[0008] The second aspect of the present disclosure provides a method for preparing the catalytic adsorbent for mercury removal and denitrification according to the first aspect of the present disclosure, comprising the following steps: (1) mixing EVS-10 molecular sieve, a cerium source and water to obtain a first mixture; (2) adding an alkaline solution to the first mixture, and then adding an alcohol to obtain a colloidal precursor; (3) performing a first calcination treatment on the colloidal precursor to obtain a first solid product; (4) mixing the first solid product, a silver source and water to perform ion exchange between the silver source and the EVS-10 molecular sieve in the first solid product; and then washing and drying to obtain a second solid product; and (5) performing a second calcination treatment on the second solid product.
[0009] Optionally, in step (1), the weight ratio of the EVS-10 molecular sieve, the cerium source and water is (85-95): (13-31): (500-600);
[0010] Optionally, the cerium source is selected from one or more of cerium acetate, cerium chloride and cerium nitrate.
[0011] Optionally, step (1) further includes: ultrasonically treating the EVS-10 molecular sieve in water for 5 to 30 minutes, and then adding the cerium source and the dispersing aid to mix to obtain the first mixture; wherein the weight ratio of the cerium source to the dispersing aid is (85 to 95): (34 to 102); preferably, the dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride, and more preferably polymethacrylic acid.
[0012] Optionally, in step (2), the alkaline solution includes aqueous ammonia; the alcohol includes ethanol; optionally, the added volume ratio of the aqueous ammonia to the alcohol is (4-12):(60-70).
[0013] Optionally, step (2) further comprises: adding an alkaline solution to the first mixture and then ultrasonically treating the mixture for 5 to 30 minutes; and
[0014] Before the first calcination treatment, the colloidal precursor is subjected to ultrasonic treatment for 5 to 30 minutes and then evaporated at 70 to 100°C.
[0015] Optionally, in step (3), the conditions of the first calcination treatment include: a calcination temperature of 350 to 600° C. and a calcination time of 1 to 4 hours;
[0016] Optionally, step (3) further comprises: cooling the product obtained after the first roasting treatment and then screening it, taking out the particles under the sieve to obtain the first solid product.
[0017] Optionally, in step (4), the silver source comprises silver nitrate; the weight ratio of the silver nitrate to the water in step (4) is 0.4-0.6:1; the weight ratio of the silver nitrate to the EVS-10 molecular sieve in step (1) is (40-60):(85-95);
[0018] Optionally, the mixing conditions include: magnetic stirring in a light-proof environment for 1 to 24 hours;
[0019] Optionally, the drying temperature is 80-110°C.
[0020] Optionally, in step (5), the conditions of the second calcination treatment include: under an inert atmosphere, a calcination temperature of 150 to 400° C., and a calcination time of 0.5 to 2 hours; the inert atmosphere is nitrogen or argon.
[0021] The third aspect of the present disclosure provides application of the catalytic adsorbent described in the first aspect of the present disclosure in the field of flue gas demercurization and denitrification; optionally, the flue gas is flue gas from a coal-fired power plant.
[0022] Through the above technical scheme, the present disclosure provides a cerium-loaded silver-loaded catalytic adsorbent for flue gas demercuration and denitrification, and its preparation method and application. The present disclosure obtains a cerium-loaded silver-loaded catalytic adsorbent based on the loading sequence of "first loading active components including CeO2, and then loading silver nanoparticles" on the EVS-10 molecular sieve, wherein the silver nanoparticles can efficiently adsorb elemental mercury; the vanadium active component in the EVS-10 molecular sieve framework can also catalytically oxidize part of the elemental mercury; the CeO2 active component has good denitrification performance and the ability to catalytically oxidize elemental mercury, and can synergistically remove elemental mercury and nitrogen oxides in coal-fired flue gas, so that the catalytic adsorbent has excellent mercury removal efficiency and high denitrification efficiency. The CeO2 active component loaded on the catalytic adsorbent EVS-10 molecular sieve has a high degree of dispersion; and the size of the silver nanoparticles can be controlled by adjusting process parameters (such as temperature, roasting atmosphere, etc.), so that the size of the silver nanoparticles can be controlled. The catalytic adsorbent provided by the present invention is relatively simple to synthesize in terms of process, can be recycled, greatly reduces the overall cost, and is suitable for industrial production; and the catalytic adsorbent has improved anti-sulfur poisoning performance, good process adaptability and compatibility, is suitable for use in series with dust removal and desulfurization equipment, and is particularly suitable for enterprises with desulfurization and dust removal equipment to expand their use for mercury removal upgrades, reduces equipment installation and use costs, and has prospects for industrial application.
[0023] Other features and advantages of the present disclosure will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0024] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0025] The inventors of the present disclosure surprisingly found in their research that simultaneously loading silver nanoparticles and active components including CeO2 on the EVS-10 molecular sieve can achieve the synergistic removal of elemental mercury and nitrogen oxides in coal-fired flue gas, and the obtained catalytic adsorbent can achieve a mercury removal efficiency of 100% and a nitrogen removal efficiency of 91%; and the inventors of the present disclosure tested the CeO2 active component for a long time in a complex flue gas environment containing SO2, and the performance showed no obvious attenuation, and it had good resistance to SO2 poisoning and a longer service life.
[0026] A first aspect of the present disclosure provides a cerium-loaded silver-loaded catalytic adsorbent for flue gas demercuration and denitrification, the catalytic adsorbent comprising a carrier and silver nanoparticles and an active component loaded on the carrier; wherein the carrier comprises an EVS-10 molecular sieve, the active component comprises CeO2, the active component is first loaded on the EVS-10 molecular sieve, and the silver nanoparticles are subsequently loaded on the EVS-10 molecular sieve.
[0027] The present disclosure obtains a cerium-loaded and silver-loaded catalytic adsorbent based on the loading sequence of "first loading active components including CeO2, then loading silver nanoparticles" on the EVS-10 molecular sieve, wherein the silver nanoparticles can efficiently adsorb elemental mercury; the vanadium active component in the EVS-10 molecular sieve framework can also catalytically oxidize part of the elemental mercury; the CeO2 active component has good denitrification performance and the ability to catalytically oxidize elemental mercury, and can synergistically remove elemental mercury and nitrogen oxides in coal-fired flue gas, so that the catalytic adsorbent has excellent mercury removal efficiency and high denitrification efficiency. The CeO2 active component loaded on the catalytic adsorbent EVS-10 molecular sieve has a high degree of dispersion; and the size of the silver nanoparticles can be controlled by adjusting process parameters (such as temperature, roasting atmosphere, etc.), so that the size of the silver nanoparticles can be controlled. The catalytic adsorbent provided by the present invention is relatively simple to synthesize in terms of process, can be recycled, greatly reduces the overall cost, and is suitable for industrial production; and the catalytic adsorbent has improved anti-sulfur poisoning performance, good process adaptability and compatibility, is suitable for use in series with dust removal and desulfurization equipment, and is particularly suitable for enterprises with desulfurization and dust removal equipment to expand their use for mercury removal upgrades, reduces equipment installation and use costs, and has prospects for industrial application.
[0028] In one embodiment, based on the total weight of the catalytic adsorbent, the mass fraction of the carrier is 45-98 weight percent, the mass fraction of the silver nanoparticles is 1-40 weight percent, and the mass fraction of the active component is 1-15 weight percent. When the content of each component in the catalytic adsorbent provided by the present disclosure is within the range of this embodiment, the catalytic adsorbent can achieve a better synergistic removal effect of elemental mercury and nitrogen oxides.
[0029] In a specific embodiment, the carrier is an EVS-10 molecular sieve, and the molar ratio of Si:Na:K:V in the EVS-10 molecular sieve is 3.92:1.39:0.48:1, based on the molar amount of the elements. Specifically, the chemical composition of the EVS-10 molecular sieve can be determined by XRF spectroscopy.
[0030] The inventors of the present disclosure also found in their research that, compared with the loading sequence of first loading silver nanoparticles on the EVS-10 molecular sieve and then loading the CeO2 active component, the loading sequence of "first loading CeO2 on the EVS-10 molecular sieve (to obtain a first solid product) and then loading silver nanoparticles on the first solid product" adopted in the present disclosure can avoid the performance degradation caused by the increase of silver nanoparticles due to secondary calcination, and can also avoid the performance degradation caused by CeO2 blocking the molecular sieve pores and causing the silver in the pores to lose its function.
[0031] The second aspect of the present disclosure provides a method for preparing the catalytic adsorbent for mercury removal and denitrification according to the first aspect of the present disclosure, comprising the following steps:
[0032] (1) mixing EVS-10 molecular sieve, a cerium source and water to obtain a first mixture;
[0033] (2) adding an alkaline solution to the first mixture, and then adding alcohol to obtain a colloidal precursor;
[0034] (3) performing a first calcination treatment on the colloidal precursor to obtain a first solid product;
[0035] (4) mixing the first solid product, a silver source and water to perform ion exchange between the silver source and the EVS-10 molecular sieve in the first solid product; then performing ion exchange, washing and drying to obtain a second solid product;
[0036] (5) performing a second calcination treatment on the second solid product.
[0037] The synthesis method provided by the present disclosure is stable and reliable, the comprehensive use cost of the catalytic adsorbent is low, and it has good prospects for industrial application.
[0038] The first solid product (EVS-10 molecular sieve loaded with CeO2) is mixed with a silver source and water, and the silver ions react with the Na + and K + In the process of ion exchange to load silver nanoparticles, the size of the silver nanoparticles can also be controlled by temperature and calcination atmosphere.
[0039] Specifically, the amount of raw material added or the weight ratio between different raw materials in the present disclosure, such as the amount or weight ratio of EVS-10 molecular sieve, cerium source and silver source, is obtained by adjusting the mass fraction of each component in the catalytic adsorbent provided in the first aspect of the present disclosure. The EVS-10 molecular sieve can be prepared according to existing methods, for example, according to the method disclosed in the document ZijianZhou, Tiantian Cao, et al. "Vanadium silicate (EVS)-supported silver nanoparticles: A novel catalytic sorbent for elemental mercury removal from flue gas". Journal of Hazardous Materials, 375 (2019) 1-8.
[0040] The EVS-10 molecular sieve used in the present disclosure can be prepared by a hydrothermal method. A specific implementation method includes: dissolving sodium silicate in deionized water; then adding NaOH, KCl, NaF and NaCl to the solution to obtain solution A. Then VOSO4 is dissolved in deionized water to obtain solution B. Solution A and solution B are mixed and stirred, and aged at room temperature. The aged mixture is transferred to an autoclave for further aging. The synthesized product is washed with deionized water and dried to obtain the EVS-10 molecular sieve. During the preparation process, the amount of each reactant and the reaction conditions can be adjusted according to actual needs.
[0041] In one embodiment, in step (1), the weight ratio of the EVS-10 molecular sieve, the cerium source and water is (85-95): (13-31): (500-600); optionally, the cerium source is selected from one or more of cerium acetate, cerium chloride and cerium nitrate.
[0042] In a preferred embodiment, step (1) further comprises: ultrasonically treating the EVS-10 molecular sieve in water for 5 to 30 minutes, and then adding the cerium source and the dispersing aid to mix to obtain the first mixture, wherein the weight ratio of the cerium source to the dispersing aid is (85 to 95): (34 to 102). The "ultrasonic treatment" described in this disclosure refers to ultrasonic treatment using a conventional ultrasonic instrument to make the material mixing or dispersion more uniform.
[0043] In a preferred embodiment, the dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride, and polymethacrylic acid is further preferred. The use of polymethacrylic acid as a dispersing aid in the present disclosure can better improve the dispersion of cerium oxide on the surface of the molecular sieve. The molecular weight of the dispersing aid in the present disclosure can vary within a large range and can be selected according to actual needs.
[0044] The inventors of the present disclosure have found that the above-mentioned dispersing aid is added to the cerium source solution, and the dispersing aid can form a complex with the cerium ion, so that the cerium ion is uniformly dispersed in the solution in the form of a complex, so that after the subsequent addition of an alkaline solution, the uniformly dispersed cerium ion complex can be stably present in the system, further avoiding the agglomeration phenomenon; after the addition of alcohol, the complex in the system forms a dispersing aid-cerium form polymer particles (such as PMAA-Ce polymer particles) on the surface of the EVS-10 molecular sieve, and the electrostatic repulsion between the particles makes the system very stable, ensuring the dispersion of the cerium ion, so that the particle size of CeO2 loaded in the finally synthesized catalytic adsorbent is small and uniformly distributed. It is beneficial to further improve the demercuration and denitration efficiency of the catalytic adsorbent.
[0045] In one embodiment, in step (2), the alkaline solution includes aqueous ammonia; the alcohol includes ethanol; further preferably, the volume ratio of the aqueous ammonia to the alcohol is (4-12): (60-70). In a specific embodiment, the mass concentration of the aqueous ammonia is 25%.
[0046] In one embodiment, step (2) further comprises: adding an alkaline solution to the first mixture and then ultrasonically treating the first mixture for 5 to 30 minutes; and before the first calcination treatment, ultrasonically treating the colloidal precursor for 5 to 30 minutes and then evaporating it at 70 to 100°C.
[0047] In one embodiment, in step (3), the conditions of the first calcination treatment include: a calcination temperature of 350 to 600° C. and a calcination time of 1 to 4 hours.
[0048] In an optional embodiment, step (3) further comprises: cooling the product obtained after the first roasting treatment and then screening it, taking the particles under the sieve to obtain the first solid product. For example, after cooling to room temperature, screening is performed using a 100-mesh sieve to take the particles under the sieve.
[0049] In one embodiment, in step (4), the silver source includes silver nitrate; the weight ratio of the silver nitrate to the water in step (4) is 0.4-0.6:1; the weight ratio of the silver nitrate to the EVS-10 molecular sieve in step (1) is (40-60):(85-95); optionally, the mixing conditions include: magnetic stirring in a light-proof environment for 1-24 hours; optionally, the drying temperature is 80-110°C.
[0050] In the present disclosure, the "light-proof environment" refers to operations well known to those skilled in the art when it comes to silver nitrate solution, such as using a brown container or wrapping it with light-proof paper in a darker environment.
[0051] In one embodiment, in step (5), in step (5), the conditions of the second calcination treatment include: under an inert atmosphere, a calcination temperature of 150 to 400° C., and a calcination time of 0.5 to 2 hours; wherein the inert atmosphere is nitrogen or argon.
[0052] The third aspect of the present disclosure provides application of the catalytic adsorbent described in the first aspect of the present disclosure in the field of flue gas demercurization and denitrification; optionally, the flue gas is flue gas from a coal-fired power plant.
[0053] The present invention is further described below in conjunction with specific embodiments, but the scope of protection claimed by the present invention is not limited to the scope described in the embodiments.
[0054] The chemicals used in each example can be obtained through public commercial channels.
[0055] The EVS-10 molecular sieve used in the following examples and comparative examples was prepared according to the method disclosed in Zijian Zhou, Tiantian Cao, et al. "Vanadium silicate (EVS)-supported silver nanoparticles: A novel catalytic sorbent for elemental mercury removal from flue gas". Journal of Hazardous Materials, 375 (2019) 1-8.
[0056] The 25% ammonia water used in the following examples, comparative examples and comparative examples is ammonia water having an NH3·H2O content of 25% by weight.
[0057] The ultrasonic treatment in the present disclosure uses a conventional ultrasonic device to make the materials mixed or dispersed more uniformly.
[0058] Example 1
[0059] (1) 9.0 g of EVS-10 molecular sieve was dispersed in 50 mL of deionized water, and after ultrasonic treatment for 15 minutes, 1.8 g of (CH3CO2)3Ce hydrate and 6.8 g of polymethacrylic acid were added;
[0060] (2) adding 8 mL of 25% ammonia water and ultrasonically treating for 15 minutes, then adding 70 mL of ethanol to form a colloidal precursor, and continuing the ultrasonic treatment for 30 minutes, evaporating the sample at 80°C, and finally calcining the sample at 500°C in a muffle furnace for 2 hours, cooling to room temperature, and sieving with a 100-mesh sieve, taking the particles under the sieve to obtain a CeO2-loaded catalyst;
[0061] (3) Weigh 4.3 g of AgNO3 and dissolve it in 100 ml of deionized water, then add the above catalyst loaded with active component CeO2, stir it magnetically in a dark environment for 6 h, then filter it, rinse it repeatedly with deionized water, dry it at 80°C, and then calcine it in a tube furnace at 250°C in a nitrogen atmosphere for 1 hour. The catalytic adsorbent loaded with CeO2 and silver nanoparticles is obtained, which is recorded as sample A.
[0062] Comparative Example 1
[0063] The catalytic adsorbent was prepared by the steps similar to those in Example 1, except that the EVS-10 molecular sieve was replaced with the commercially available ETS-10 molecular sieve. The other preparation steps and reaction conditions were the same as those in Example 1, and a catalytic adsorbent loaded with CeO2 and silver nanoparticles was obtained, which was recorded as sample D-1.
[0064] Example 2
[0065] (1) 9.5 g of EVS-10 molecular sieve was dispersed in 60 mL of deionized water, and then ultrasonicated for 15 min and then 1.3 g of Ce(NO3)3·6H2O and 3.4 g of polymethacrylic acid were added;
[0066] (2) adding 4 mL of 25% ammonia water and ultrasonically treating for 15 minutes, then adding 60 mL of ethanol to form a colloidal precursor, and continuing the ultrasonic treatment for 30 minutes, evaporating the sample at 80°C, and finally calcining the sample at 600°C in a muffle furnace for 2 hours, cooling to room temperature, and sieving with a 100-mesh sieve, taking the particles under the sieve to obtain a CeO2-loaded catalyst;
[0067] (3) Weigh 6.0 g of AgNO3 and dissolve it in 100 ml of deionized water. Then add the above-mentioned catalyst loaded with active component CeO2, stir it magnetically in a light-proof environment for 24 h, then filter it, rinse it repeatedly with deionized water, dry it at 100°C, and then calcine it in a tube furnace at 300°C in an argon atmosphere for 1 hour to obtain a catalytic adsorbent loaded with CeO2 and silver nanoparticles, which is recorded as sample B.
[0068] Example 3
[0069] (1) 8.5 g of EVS-10 molecular sieve was dispersed in 60 mL of deionized water, and then ultrasonicated for 15 min before adding 3.1 g of CeCl3·6H2O and 10.2 g of polymethacrylic acid;
[0070] (2) adding 12 mL of 25% ammonia water and ultrasonically treating for 15 minutes, then adding 70 mL of ethanol to form a colloidal precursor, and continuing the ultrasonic treatment for 30 minutes, evaporating the sample at 80°C, and finally calcining the sample at 550°C in a muffle furnace for 2 hours, cooling to room temperature, and sieving with a 100-mesh sieve, taking the particles under the sieve to obtain a CeO2-loaded catalyst;
[0071] (3) Weigh 4.3 g of AgNO3 and dissolve it in 100 ml of deionized water, then add the above catalyst loaded with active component CeO2, stir it magnetically in a dark environment for 8 h, then filter it, rinse it repeatedly with deionized water, dry it at 80°C, and then calcine it in a tube furnace at 300°C in a nitrogen atmosphere for 1 hour. The catalytic adsorbent loaded with CeO2 and silver nanoparticles is obtained, which is recorded as sample C.
[0072] Example 4
[0073] (1) 9.5 g of EVS-10 molecular sieve was dispersed in 60 mL of deionized water, and then ultrasonicated for 15 min and 1.3 g of Ce(NO3)3·6H2O was added;
[0074] (2) adding 4 mL of 25% ammonia water and ultrasonically treating for 15 minutes, then adding 60 mL of ethanol to form a colloidal precursor, and continuing the ultrasonic treatment for 30 minutes, evaporating the sample at 80°C, and finally calcining the sample at 600°C in a muffle furnace for 2 hours, cooling to room temperature, and sieving with a 100-mesh sieve, taking the particles under the sieve to obtain a CeO2-loaded catalyst;
[0075] (3) Weigh 6 g of AgNO3 and dissolve it in 100 ml of deionized water. Then add the above-mentioned catalyst loaded with active component CeO2, stir it magnetically in a light-proof environment for 24 h, then filter it, rinse it repeatedly with deionized water, dry it at 100°C, and then calcine it in a tube furnace at 300°C in an argon atmosphere for 1 hour to obtain a catalytic adsorbent loaded with CeO2 and silver nanoparticles, which is recorded as sample D.
[0076] Comparative Example 2
[0077] Weigh 4.3 g of AgNO3 and dissolve it in 100 ml of deionized water, then add 10 g of EVS-10 molecular sieve, stir it magnetically in a dark environment for 6 h, then filter it, rinse it repeatedly with deionized water, dry it at 80 ° C, and then bake it in a tube furnace at 250 ° C in a nitrogen atmosphere for 1 hour. The catalytic adsorbent loaded with only silver nanoparticles is obtained, which is recorded as sample D-2.
[0078] The mass fractions of the various components in the samples prepared in the above examples and comparative examples are listed in the following Table 1.
[0079] Table 1
[0080]
[0081] Among them, in the catalytic adsorbent, the molar amount of cerium element is determined according to the added amount of raw material cerium source, and then the mass of CeO2 is determined according to the molar amount of cerium element; the molar amount of silver element is determined according to the added amount of raw material silver source, and then the mass of silver particles is determined according to the molar amount of silver element; the mass fraction of each component is calculated based on the calculated mass of CeO2 and silver particles and the total mass of the added EVS-10 molecular sieve as the final adsorption catalyst. (Due to the small sample loss, it is ignored in the calculation)
[0082] Simulated smoke test example
[0083] The samples synthesized in the above embodiments, comparative examples and comparative examples were placed in an experimental system simulating flue gas to test the demercuration and denitrification performance. The simulated flue gas conditions are as follows: 5% O2, 12% CO2, 400ppm NO, 400ppm NH3, 600ppm SO2, 30ppm HCl, Hg 0 Concentration: 110 μg / m 3 The balance gas is N2, and the total flow rate of the simulated flue gas is 500 mL / min. The experimental system for simulating flue gas can be a conventional experimental system in the art. The results of the mercury removal and denitrification tests are listed in Table 2 below.
[0084] Table 2
[0085]
[0086]
[0087] According to Table 2 above, by comparing Example 1 with Comparative Example 1, it can be seen that compared with the commercially available ETS-10 molecular sieve used in Comparative Example 1, the Hg content of the catalyst prepared by using EVS-10 molecular sieve in Example 1 is 0 Removal efficiency and NO x The removal efficiency is better.
[0088] Comparing Examples 1 to 4 of the present application with Comparative Example 2, the catalytic adsorbent samples prepared by the method provided by the present disclosure in Examples 1 to 4 can simultaneously remove Hg 0 and NO x .
[0089] Furthermore, by comparing Examples 1 to 3 with Example 4, it can be seen that the addition of a dispersing agent in Examples 1 to 3 results in a catalytic adsorbent having a higher Hg 0 Removal efficiency and NO x Removal efficiency.
[0090] The preferred embodiments of the present disclosure are described in detail above; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0091] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0092] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A cerium-supported silver-supported catalytic adsorbent for flue gas demercuration and denitrification, characterized in that: The catalytic adsorbent comprises a carrier, silver nanoparticles and active components loaded on the carrier; wherein the carrier comprises an EVS-10 molecular sieve, the active component comprises CeO2, the active component is first loaded on the EVS-10 molecular sieve, and the silver nanoparticles are then loaded on the EVS-10 molecular sieve; The catalytic adsorbent is prepared by a method comprising the following steps: (1) mixing EVS-10 molecular sieve, a cerium source and water to obtain a first mixture; (2) adding an alkaline solution to the first mixture, and then adding alcohol to obtain a colloidal precursor; (3) performing a first calcination treatment on the colloidal precursor to obtain a first solid product; (4) mixing the first solid product, a silver source and water to perform ion exchange between the silver source and the EVS-10 molecular sieve in the first solid product; then washing and drying to obtain a second solid product; (5) performing a second roasting treatment on the second solid product; Wherein step (1) further comprises: subjecting the EVS-10 molecular sieve to ultrasonic treatment in water for 5 to 30 minutes, and then adding the cerium source and the dispersing aid to mix, so as to obtain the first mixture; the dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride.
2. The catalytic adsorbent according to claim 1, characterized in that: Based on the total weight of the catalytic adsorbent, the mass fraction of the carrier is 45-98 weight %, the mass fraction of the silver nanoparticles is 1-40 weight %, and the mass fraction of the active component is 1-15 weight %.
3. The catalytic adsorbent according to claim 1, characterized in that: In step (1), the weight ratio of the EVS-10 molecular sieve, the cerium source and water is (85-95): (13-31): (500-600).
4. The catalytic adsorbent according to claim 1, characterized in that: The cerium source is selected from one or more of cerium acetate, cerium chloride and cerium nitrate.
5. The catalytic adsorbent according to claim 1, characterized in that: The weight ratio of the cerium source to the dispersing aid is (85-95): (34-102).
6. The catalytic adsorbent according to claim 1, characterized in that: The dispersing aid is polymethacrylic acid.
7. The catalytic adsorbent according to claim 1, characterized in that: In step (2), the alkaline solution includes aqueous ammonia; and the alcohol includes ethanol.
8. The catalytic adsorbent according to claim 7, characterized in that: The added volume ratio of the ammonia water to the alcohol is (4-12): (60-70).
9. The catalytic adsorbent according to claim 1, characterized in that: Step (2) also includes: Adding an alkaline solution to the first mixture and then ultrasonically treating for 5 to 30 minutes; and Before the first calcination treatment, the colloidal precursor is ultrasonically treated for 5 to 30 minutes and then evaporated at 70 to 100°C.
10. The catalytic adsorbent according to claim 1, characterized in that: In step (3), the conditions of the first calcination treatment include: a calcination temperature of 350-600° C. and a calcination time of 1-4 hours.
11. The catalytic adsorbent according to claim 1, characterized in that: Step (3) also includes: cooling the product obtained after the first roasting treatment and then screening it, taking out the particles under the sieve to obtain the first solid product.
12. The catalytic adsorbent according to claim 1, characterized in that: In step (4), the silver source includes silver nitrate; the weight ratio of the silver nitrate to the water in step (4) is 0.4-0.6:1; the weight ratio of the silver nitrate to the EVS-10 molecular sieve in step (1) is (40-60):(85-95).
13. The catalytic adsorbent according to claim 1, characterized in that: In step (4), the mixing conditions include: magnetic stirring for 1 to 24 hours in a light-proof environment; and the drying temperature is 80 to 110°C.
14. The catalytic adsorbent according to claim 1, characterized in that: In step (5), the conditions of the second calcination treatment include: in an inert atmosphere, a calcination temperature of 150-400° C., and a calcination time of 0.5-2 hours; the inert atmosphere is nitrogen or argon.
15. Use of the cerium-supported silver-supported catalytic adsorbent according to any one of claims 1 to 14 in the field of flue gas mercury removal and denitrification.
16. The use according to claim 15, characterized in that The flue gas is flue gas from a coal-fired power plant.