A catalyst for dehydrogenating low-carbon alkanes to produce olefins, and its preparation method and application

By using low-carbon alkane dehydrogenation catalysts with components such as ZnO, zirconia and silicon oxide, the problems of rapid catalyst deactivation and environmental pollution are solved, and the efficiency and low cost of propylene production are achieved, meeting the rapidly growing demand.

CN116059991BActive Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111273296.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-11-12
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

In the existing propylene production process, the catalyst deactivation is fast, the cost is high, the environmental pollution risk is high, and it is difficult to meet the rapidly growing propylene demand.

Method used

Used with 20-50% ZnO, 20-65% of the first additive component (zirconium dioxide and silica composite oxide) and 0.1-10% of the second additive component (lithium, sodium, potassium) , oxides of magnesium and barium) and 10-50% binder low-carbon alkane dehydrogenation catalyst were prepared by drying and calcining treatment and used for propane dehydrogenation reaction.

Benefits of technology

It improves the activity and selectivity of the catalyst, reduces costs, has good industrial application prospects, and improves the yield of propylene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003329348540000111
    Figure BDA0003329348540000111
  • Figure BDA0003329348540000112
    Figure BDA0003329348540000112
  • Figure BDA0003329348540000121
    Figure BDA0003329348540000121
Patent Text Reader

Abstract

The present invention relates to a catalyst for the dehydrogenation of low-carbon alkanes to produce olefins, a preparation method thereof and an application thereof. The catalyst contains 20-50% by weight of ZnO, 20-65% by weight of a first auxiliary component, 0.1-10% by weight of a second auxiliary component and 10-50% by weight of a binder, based on the dry weight of the catalyst; wherein the first auxiliary component contains a composite oxide of zirconium dioxide and silicon dioxide and a first metal element, the first metal element being selected from one or more of titanium, manganese, tin and tungsten; and the second auxiliary component contains a second metal element, the second metal element being selected from one or more of lithium, sodium, potassium, magnesium, barium and calcium. The catalyst of the present invention has high reaction activity, and is used for the dehydrogenation of low-carbon olefins to produce olefins with high conversion rate and selectivity of target products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a catalyst for dehydrogenating low-carbon alkanes to produce olefins, and a preparation method and application thereof. Background Art

[0002] Propylene is one of the basic chemical raw materials and is widely used in the synthesis of various chemical products such as polypropylene, propylene oxide, acrylic acid and acrylonitrile. At present, propylene is mainly produced from co-production or by-products of processes such as naphtha cracking and catalytic cracking. However, with the increasing consumption of propylene year by year, traditional propylene production can no longer meet the demand. Therefore, the technology of producing propylene by dehydrogenation of propane has developed rapidly. The industrialized process technologies for producing propylene by catalytic dehydrogenation of propane mainly include UOP's Oleflex technology and Lummus's Catofin technology. The Oleflex process uses a moving bed reactor with continuous catalyst regeneration, with Pt-Sn / Al2O3 as the catalyst, and K or Li is added for modification; the Catofin process uses a fixed bed reactor with Cr2O3 / Al2O3 as the catalyst. The catalyst deactivates quickly and needs to be regenerated every 15 minutes.

[0003] Compared with the above two processes, the fluidized bed propane dehydrogenation process adopts a single reactor design, which can realize the continuous input and output of solid materials, facilitate the continuous regeneration and circulation operation of the catalyst, and has flexible operating devices, good operating flexibility and raw material adaptability. In addition, the vigorous stirring of the catalyst and the raw material promotes the mass transfer and heat transfer process. The movement of the fluid and particles makes the bed have good heat transfer performance, and the temperature inside the bed is uniform, which is conducive to the full play of the catalyst activity. The FBD fluidized bed dehydrogenation process jointly developed by the Yaroslavl Research Institute of Russia and Snamprogetti Engineering Company of Italy was industrialized in 1964. The catalyst used is microsphere Cr2O3 / Al2O3, but there is also a high risk of catalyst environmental pollution and difficulty in handling. Therefore, it is of great significance to develop a propane dehydrogenation catalyst with high activity, low cost and green environmental protection.

[0004] CN102451677B discloses a catalyst for isobutane dehydrogenation, wherein the catalyst uses one or more oxides of MgO, P2O5, ZrO2, Al2O3 or SiO2 as carriers, one or more oxides of Ti, Nb, Ta, W, Re, In or Ga as active components, and uses a continuous reaction-regeneration device to dehydrogenate isobutane to olefins. However, the catalyst is easily deactivated, the reaction device is expensive, and the presence of sulfur causes great loss to the device.

[0005] CN105618026A discloses a catalyst for dehydrogenation of alkanes, and a preparation method and a use method thereof. The catalyst comprises a dehydrogenation active component, a carrier and a second auxiliary agent. The dehydrogenation active component is one or more metals or oxides of Fe, Zn, Cu, Ga and Pb, with a content of 0.1 to 60 parts, preferably 2 to 20 parts; the carrier is a mixed oxide or composite oxide formed by one or more of SiO2, Al2O3, ZrO2, MgAl2O4 and ZnAl2O4, or a molecular sieve, with a content of 40 to 99.9 parts, preferably 80 to 98 parts.

[0006] CN108727148B discloses a highly dispersed ZnO-based catalyst and its preparation method and a propane oxygen-free dehydrogenation method. The catalyst uses Silicalite-1 as a carrier, ZIF-8 as a precursor of ZnO and a precursor of a carbon material, and forms highly dispersed ZnO nanoparticles coated with carbon materials during high-temperature pyrolysis; by further leaching with nitric acid, smaller ZnO nanoparticles can be obtained, thereby improving the stability of the catalyst.

[0007] CN110614092A discloses a non-precious metal propane dehydrogenation catalyst and a preparation method thereof. The catalyst active component is at least one of iron, nickel, zinc, molybdenum, tungsten, manganese, tin, copper and their respective oxides, which is impregnated on a sulfur-modified alumina carrier to obtain a non-precious metal propane dehydrogenation catalyst.

[0008] CN112619686A discloses a supported non-precious metal dehydrogenation catalyst and its preparation method and application. The active component of the catalyst is zinc and / or zinc oxide, the auxiliary agent is phosphorus and / or phosphorus oxide, and the carrier is MFI molecular sieve. The MFI molecular sieve synthesized by hydrothermal method is treated with alkali to improve the pore structure, and at the same time, the content of active components and auxiliary agents in the molecular sieve pores is increased by vacuum impregnation. The limiting effect of the pore size can reduce the aggregation of active components such as Zn and extend the service life of the catalyst.

[0009] CN110801861 discloses an environmentally friendly propane direct dehydrogenation catalyst for producing propylene, and a method for preparing the catalyst. The catalyst comprises 30% to 70% Zn-doped Hβ molecular sieve, 15% to 50% Al2O3, and 3% to 30% multi-element active modifier. The modifier is a first modifier of at least one element among W, Mo, Mn, Zr, Ni, Fe, and Co, a second modifier of at least one element among Ga, In, P, La, and Ce, and a third modifier of any one element among Sr, Ba, Ca, Mg, Na, and Li. The fluidized bed dehydrogenation catalyst has low cost and good wear resistance, and has good dehydrogenation activity and stability for propane dehydrogenation. Summary of the invention

[0010] The purpose of the present invention is to provide a catalyst for dehydrogenating low-carbon alkanes to olefins, and a preparation method and application thereof. The catalyst of the present invention is low-cost and environmentally friendly, has excellent activity and selectivity, and can improve the yield of the target product propylene.

[0011] In order to achieve the above object, the first aspect of the present invention provides a catalyst for dehydrogenating low-carbon alkanes to olefins, which comprises, based on the dry weight of the catalyst, 20-50 wt% of ZnO, 20-65 wt% of a first auxiliary component, 0.1-10 wt% of a second auxiliary component and 10-50 wt% of a binder;

[0012] Wherein, the first auxiliary agent component contains a composite oxide of zirconium dioxide and silicon dioxide and a first metal element, and the first metal element is selected from one or more of titanium, manganese, tin and tungsten;

[0013] The second auxiliary agent component contains a second metal element, and the second metal element is selected from one or more of lithium, sodium, potassium, magnesium, barium and calcium.

[0014] Optionally, the catalyst contains 20-45 wt % of the ZnO, 20-50 wt % of the first auxiliary component, 0.1-8 wt % of the second auxiliary component and 10-40 wt % of the binder.

[0015] Optionally, the content of silicon dioxide in the composite oxide of zirconium dioxide and silicon dioxide is 0.1-50% by weight, preferably 0.1-30% by weight.

[0016] Optionally, the first auxiliary agent component contains a composite oxide of zirconium dioxide and silicon dioxide and an oxide of the first metal element; and the second auxiliary agent component contains a chloride of the second metal element.

[0017] Optionally, the binder is selected from one or more of aluminum sol, silica sol and SB powder.

[0018] The second aspect of the present invention provides a method for preparing the catalyst provided in the first aspect of the present invention, the method comprising: mixing a zinc source, a zirconium dioxide and silicon dioxide composite oxide, a first metal source, a second metal source, a binder and a solvent, and then drying and calcining the obtained mixture.

[0019] Optionally, the zinc source is a soluble zinc salt and / or zinc oxide;

[0020] The first metal source contains an oxide of a first metal element, preferably one or more of titanium oxide, manganese oxide, tin oxide and tungsten oxide;

[0021] The second metal source contains an oxide of a second metal element, preferably one or more of lithium chloride, sodium chloride, potassium chloride, magnesium chloride, barium chloride and calcium chloride;

[0022] The solvent is selected from one or more of methanol, ethanol and water.

[0023] Optionally, the mixing conditions include: temperature of 20-40°C, time of 10-60 min; preferably, temperature of 20-30°C, time of 20-40 min.

[0024] Optionally, the drying conditions include: a temperature of 30-180° C. and a time of 1-24 hours; preferably, a temperature of 90-130° C. and a time of 5-15 hours.

[0025] Optionally, the calcination conditions include: a temperature of 600-1100° C. and a time of 1-10 hours; preferably a temperature of 600-850° C. and a time of 1-7 hours;

[0026] More preferably, the calcination includes a first calcination and a second calcination performed sequentially; the conditions of the first calcination include: a temperature of 600-850°C and a time of 1-7 hours; the conditions of the second calcination include: a temperature of 800-1100°C and a time of 1-7 hours.

[0027] The third aspect of the present invention provides a method for dehydrogenating low-carbon alkanes to produce olefins, the method comprising: contacting low-carbon alkanes with the catalyst provided by the first aspect of the present invention to carry out a dehydrogenation reaction.

[0028] Optionally, the conditions for the dehydrogenation reaction include: the mass space velocity of the light alkane is 0.1-10h -1 The reaction temperature is 550-650°C and the reaction pressure is 0.01-0.1MPa; the low carbon alkane is selected from propane, butane or isobutane.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) Using zinc as the active component of the propane dehydrogenation catalyst, the activity and selectivity of the catalyst can be improved by using the first auxiliary agent and the second auxiliary agent in combination, and the use of zinc as the active component of the propane dehydrogenation catalyst can improve the yield of the target olefin product by using the catalyst for the dehydrogenation of low-carbon alkanes to olefins;

[0031] (2) The catalyst of the present invention has no stringent requirements on the carrier, has the advantage of low price, and has good industrial application prospects.

[0032] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0033] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0034] The first aspect of the present invention provides a catalyst for dehydrogenating low-carbon alkanes to produce olefins. Based on the dry weight of the catalyst, the catalyst contains 20-50 weight percent of ZnO, 20-65 weight percent of a first auxiliary component, 0.1-10 weight percent of a second auxiliary component and 10-50 weight percent of a binder; wherein the first auxiliary component contains a composite oxide of zirconium dioxide and silicon dioxide and a first metal element, and the first metal element is selected from one or more of titanium, manganese, tin and tungsten; and the second auxiliary component contains a second metal element, and the second metal element is selected from one or more of lithium, sodium, potassium, magnesium, barium and calcium.

[0035] The catalyst of the present invention uses zinc as the active component of the catalyst propane dehydrogenation, and can improve the activity and selectivity of the catalyst by using the first auxiliary agent and the second auxiliary agent in combination. The catalyst can be used in the process of dehydrogenating light olefins to produce propane to improve the selectivity of the target product.

[0036] In a specific embodiment of the present invention, the catalyst contains 20-45 wt % of the ZnO, 20-50 wt % of the first auxiliary component, 0.1-8 wt % of the second auxiliary component and 10-40 wt % of the binder.

[0037] In a specific embodiment of the present invention, the content of silicon dioxide in the composite oxide of zirconium dioxide and silicon dioxide is 0.1-50% by weight, preferably 0.1-30% by weight, and more preferably 0.1-20% by weight.

[0038] In a specific embodiment of the present invention, the first auxiliary component contains a composite oxide of zirconium dioxide and silicon dioxide and an oxide of the first metal element, and the oxide of the first metal element may be, for example, one or more of titanium oxide, manganese oxide, tin oxide and tungsten oxide; the second auxiliary component contains an oxide of the second metal element, such as lithium chloride, sodium chloride, potassium chloride, magnesium chloride, barium chloride and calcium chloride.

[0039] In a specific embodiment of the present invention, the binder is selected from one or more of aluminum sol, silica sol and SB powder, preferably aluminum sol and / or SB powder.

[0040] The second aspect of the present invention provides a method for preparing the catalyst provided in the first aspect of the present invention, the method comprising: mixing a zinc source, a zirconium dioxide and silicon dioxide composite oxide, a first metal source, a second metal source, a binder and a solvent, and then drying and calcining the obtained mixture.

[0041] The method of the invention has a simple production process and is environmentally friendly, and can prepare a catalyst with relatively excellent reaction activity.

[0042] In a preferred embodiment of the present invention, the mixing conditions include: temperature of 20-40°C, time of 10-60 min; preferably, temperature of 20-30°C, time of 20-40 min.

[0043] In a preferred embodiment of the present invention, the method comprises: firstly mixing the zinc source, zirconium dioxide and silicon dioxide composite oxide, the first metal source, the second metal source and the solvent, and then adding the binder for second mixing. The conditions of the first mixing include: temperature of 20-40°C and time of 1-30min; the conditions of the second mixing include: temperature of 20-40°C and time of 1-30min.

[0044] In a specific embodiment of the present invention, the zinc source is a soluble zinc salt and / or zinc oxide, for example, it can be selected from one or more of zinc oxide, zinc chloride, zinc nitrate, zinc acetate and zinc carbonate; the first metal source contains an oxide of a first metal element, preferably one or more of titanium oxide, manganese oxide, tin oxide and tungsten oxide; the second metal source contains an oxide of a second metal element, preferably one or more of lithium chloride, sodium chloride, potassium chloride, magnesium chloride, barium chloride and calcium chloride; the solvent is water.

[0045] In a specific embodiment of the present invention, the mixing conditions include: temperature of 20-40°C, time of 10-60 min; preferably, temperature of 20-30°C, time of 20-40 min. More preferably, the mixing is carried out under stirring, and the stirring can be carried out by a device conventionally used by those skilled in the art, such as a mechanical stirrer.

[0046] In a specific embodiment of the present invention, the drying conditions include: a temperature of 30-180°C and a time of 1-24 hours; preferably, a temperature of 90-130°C and a time of 5-15 hours. Drying is well known to those skilled in the art, for example, it can be carried out in a constant temperature drying oven or a tube furnace.

[0047] In a specific embodiment of the present invention, the conditions for calcination include: a temperature of 600-1100°C and a time of 1-10 hours; preferably, the temperature is 600-850°C and the time is 1-7 hours. The present invention does not specifically limit the atmosphere for calcination, for example, it can be an air atmosphere. Calcination is well known to those skilled in the art and can be carried out in a device conventionally used by those skilled in the art, for example, a muffle furnace or a tube furnace can be used. In a preferred embodiment, the calcination includes a first calcination and a second calcination carried out in sequence; the temperature of the first calcination is lower than the temperature of the second calcination. Preferably, the conditions for the first calcination include: a temperature of 600-850°C and a time of 1-7 hours; the conditions for the second calcination include: a temperature of 800-1100°C and a time of 1-7 hours. Staged calcination is conducive to the preparation of a catalyst with better reaction activity.

[0048] The third aspect of the present invention provides a method for producing olefins by dehydrogenating low-carbon alkanes, the method comprising: contacting low-carbon alkanes with the catalyst provided by the first aspect of the present invention to carry out a dehydrogenation reaction. The method of the present invention has a relatively good selectivity for low-carbon alkanes.

[0049] In a specific embodiment of the present invention, the conditions for the dehydrogenation reaction include: the mass space velocity of the light alkane is 0.1-10h -1 The reaction temperature is 550-650°C and the reaction pressure is 0.01-0.1MPa; the low carbon alkane is selected from propane, butane or isobutane.

[0050] The present invention is further illustrated by the following examples, but the present invention is not limited thereto.

[0051] In the following examples and comparative examples, unless otherwise specified, all reagents used are commercially available. The silicon dioxide and zirconium dioxide composite oxides were prepared by the following method:

[0052] (1) Preparation of zirconium hydroxide.

[0053] Take a 5% zirconium oxychloride (ZrOCl2·8H2O) aqueous solution, slowly add 25% ammonia water while stirring, adjust the pH to 9, transfer the resulting zirconium hydroxide precipitate and the solution to an autoclave, seal it, and hydrothermally treat it at 100°C for 24 hours. Filter and wash the solid with deionized water until there is no Cl in the filtrate. - , and dried at 110°C for 24 hours to obtain zirconium hydroxide powder.

[0054] (2) Preparation of zirconium dioxide and silicon dioxide composite oxide

[0055] Take 40 grams of the zirconium hydroxide powder prepared above, add it to 150 ml of aqueous solution and stir, add 16.8 grams of silica sol (produced by Changzhou Jinfeng Chemical Co., Ltd.), whose SiO2 content is 42% by mass, the colloidal particle size is 10nm, the pH value is 8.5, and the Na2O content is 0.05% by mass. After mixing evenly, dry at 110°C for 24 hours and calcine at 800°C for 3 hours.

[0056] Example 1

[0057] Take 6g of zinc oxide, 6g of titanium oxide, 1.4g of silicon dioxide and zirconium dioxide composite oxide (silicon dioxide content is 1.5 weight%) and 0.3812g of magnesium chloride, add them into 35mL of deionized water and stir evenly, then add 21.21g of aluminum sol into the slurry and mix and stir at 30°C for 40min until it is fixed. The obtained mixture is dried at 120°C for 12h, then calcined at 600°C in air atmosphere for 1h, and then calcined at 815°C in air atmosphere for 4h to obtain catalyst A. The composition of the catalyst is shown in Table 1, the same below.

[0058] Example 2

[0059] Take 6g of zinc oxide, 6g of titanium oxide, 1.4g of silica and zirconium dioxide composite oxide (silicon dioxide content is 1.5 weight%) and 0.1288g of calcium chloride, add them into 35mL of deionized water and stir evenly, then add 21.21g of aluminum sol into the slurry and mix and stir at 30°C for 40min. The obtained mixture is dried at 120°C for 12h, then calcined at 600°C in air atmosphere for 1h, and then calcined at 815°C in air atmosphere for 4h to obtain catalyst B.

[0060] Example 3

[0061] Catalyst C was prepared in the same manner as in Example 1, except that the mass of magnesium chloride added was 0.2300 g.

[0062] Example 4

[0063] Catalyst D was prepared in the same manner as in Example 1, except that 0.4577 g of magnesium chloride was added.

[0064] Example 5

[0065] Catalyst E was prepared in the same manner as in Example 1, except that 6 g of tungsten oxide was used instead of 6 g of titanium oxide, and 0.0869 g of potassium chloride was used instead of 0.3812 g of magnesium chloride.

[0066] Example 6

[0067] Catalyst F was prepared in the same manner as in Example 1, except that 6 g of manganese oxide was used instead of 6 g of titanium oxide.

[0068] Example 7

[0069] Catalyst G was prepared in the same manner as in Example 1, except that the content of silicon dioxide in the composite oxide of silicon dioxide and zirconium dioxide was 35 wt %.

[0070] Comparative Example 1

[0071] 6g of zinc oxide, 6g of titanium oxide and 1.4g of silicon dioxide and zirconium dioxide composite oxide (the content of silicon dioxide is 1.5% by weight) are added to 35mL of deionized water and stirred evenly, and then 21.21g of aluminum sol is added to the slurry and mixed and stirred at 30°C for 40min until it is fixed, and the obtained mixture sample is dried at 120°C for 12h, then calcined at 600°C in an air atmosphere for 1h, and then calcined at 815°C in a muffle furnace for 4h to obtain catalyst a. The prepared catalyst a contains 33.4% by weight of zinc oxide, 41.2% by weight of the first auxiliary component, 25.4% by weight of a binder, and does not contain the second auxiliary component.

[0072] Comparative Example 2

[0073] Catalyst b was prepared in the same manner as in Example 1, except that 1.4 g of silicon dioxide was used instead of 1.4 g of silicon dioxide and zirconium dioxide composite oxide. The prepared catalyst b contained 33.4 wt % of zinc oxide, 41.2 wt % of the first auxiliary component, 0.4 wt % of the second auxiliary component, and 25.4 wt % of a binder.

[0074] Comparative Example 3

[0075] 2.0476 g of zinc nitrate was mixed with 20 mL of deionized water to prepare an impregnation solution, and the catalyst was prepared by impregnation. 15 g of zirconium oxide was used as a carrier, and it was contacted with the impregnation solution for impregnation, with a liquid-to-solid mass ratio of 1.2. After impregnation, it was rotary evaporated to dryness at 75°C and a vacuum degree of -0.08 MPa, dried at 120°C for 12 hours, and then calcined at 700°C for 4 hours to obtain catalyst c. The prepared catalyst c contains 3% by weight of zinc element.

[0076] Comparative Example 4

[0077] 2.6 g of zinc nitrate and 1.7 g of anhydrous zirconium chloride were dissolved in 500 mL of chilled water, 24 mL of titanium tetrachloride was added with stirring, and ammonia water was added dropwise at 55° C. until the pH value of the solution was neutral, aged for 2 h, the precipitate was filtered and dried for 12 h, and then calcined at 700° C. for 4 h to obtain catalyst d. The prepared catalyst d contained 6.1% by weight of zinc oxide, 86.3% by weight of titanium oxide, and 7.7% by weight of zirconium oxide.

[0078] Comparative Example 5

[0079] Catalyst e was prepared in the same manner as in Example 1, except that 12.23 g of zinc oxide was added.

[0080] Test Case

[0081] In the microreactor, 3 g of catalyst was loaded, propane was used as the raw material, and the propane feed mass space velocity was 3.5 h-1 at 620 °C, atmospheric pressure, and 1.5 h-1. -1 The propane dehydrogenation reaction was carried out under the conditions of , and propane was introduced for 5 minutes for sampling. The propane conversion rate and propylene selectivity were calculated. The changes in the propane dehydrogenation reaction conversion rate, the changes in the propylene selectivity, the changes in the propylene yield and the carbon deposit content are shown in Table 2.

[0082] Table 1

[0083]

[0084] Table 2

[0085]

[0086]

[0087] It can be seen from the above results that the dehydrogenation catalyst prepared by the method of the present invention has both high propane conversion rate and propylene selectivity.

[0088] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0089] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0090] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A catalyst for dehydrogenating low carbon alkanes to olefins, comprising, based on the dry weight of the catalyst, 20-50 wt % of ZnO, 20-65 wt % of a first auxiliary component, 0.1-10 wt % of a second auxiliary component and 10-50 wt % of a binder; in, The first auxiliary agent component contains a composite oxide of zirconium dioxide and silicon dioxide and a first metal element, wherein the first metal element is selected from one or more of titanium, manganese and tungsten; The second auxiliary agent component contains a second metal element, and the second metal element is selected from one or more of lithium, sodium, potassium, magnesium, barium and calcium.

2. The catalyst according to claim 1, wherein The catalyst contains 20-45 wt % of the ZnO, 20-50 wt % of the first auxiliary component, 0.1-8 wt % of the second auxiliary component and 10-40 wt % of the binder.

3. The catalyst according to claim 1, wherein The content of silicon dioxide in the composite oxide of zirconium dioxide and silicon dioxide is 0.1-50% by weight.

4. The catalyst according to claim 1, wherein The content of silicon dioxide in the composite oxide of zirconium dioxide and silicon dioxide is 0.1-30% by weight.

5. The catalyst according to claim 1, wherein The first auxiliary agent component contains a composite oxide of zirconium dioxide and silicon dioxide and an oxide of the first metal element; The second auxiliary component contains a chloride of the second metal element.

6. The catalyst according to claim 1, wherein The binder is selected from one or more of aluminum sol, silica sol and SB powder.

7. A method for preparing the catalyst according to any one of claims 1 to 6, the method comprising: After mixing a zinc source, a composite oxide of zirconium dioxide and silicon dioxide, a first metal source, a second metal source, a binder and a solvent, the obtained mixture is dried and calcined.

8. The method according to claim 7, wherein: The zinc source is a soluble zinc salt and / or zinc oxide; The first metal source contains an oxide of a first metal element; The second metal source contains a chloride of a second metal element; The solvent is selected from one or more of methanol, ethanol and water.

9. The method according to claim 8, wherein: The first metal source contains one or more of titanium oxide, manganese oxide and tungsten oxide; The second metal source contains one or more of lithium chloride, sodium chloride, potassium chloride, magnesium chloride, barium chloride and calcium chloride.

10. The method according to claim 7, wherein: The mixing conditions include: temperature of 20-40° C. and time of 10-60 min.

11. The method according to claim 10, wherein: The mixing conditions include: temperature of 20-30° C. and time of 20-40 min.

12. The method according to claim 7, wherein: The drying conditions include: a temperature of 30-180° C. and a time of 1-24 hours.

13. The method according to claim 12, wherein: The drying conditions include: a temperature of 90-130° C. and a drying time of 5-15 hours.

14. The method according to claim 7, wherein: The calcination conditions include: a temperature of 600-1100° C. and a time of 1-10 hours.

15. The method according to claim 14, wherein: The calcination conditions include: a temperature of 600-850° C. and a time of 1-7 hours.

16. The method according to claim 14, wherein: The roasting includes a first roasting and a second roasting performed sequentially; The conditions for the first calcination include: a temperature of 600-850° C. and a time of 1-7 hours; the conditions for the second calcination include: a temperature of 800-1100° C. and a time of 1-7 hours.

17. A method for dehydrogenating low-carbon alkanes to produce olefins, the method comprising: The low carbon alkane is contacted with the catalyst according to any one of claims 1 to 6 to carry out a dehydrogenation reaction.

18. The method according to claim 17, wherein: The conditions for the dehydrogenation reaction include: the mass space velocity of the light alkane is 0.1-10h -1 , the reaction temperature is 550-650℃, and the reaction pressure is 0.01-0.1MPa; The low carbon alkane is selected from propane, butane or isobutane.