Aluminum sol and its preparation method and application

By adopting specific temperature and pH adjustment methods in the preparation of aluminum sol, an aluminum sol with high aluminum-chlorine mass ratio is prepared, which solves the problems of high preparation cost of aluminum sol and blockage of active components in the prior art, and improves the catalyst adhesion and cracking properties.

CN116060044BActive Publication Date: 2024-12-06CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111271117.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-12-06
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

The existing aluminum sol preparation methods have problems such as high production costs, high safety risks, high raw materials, flammable and easy to corrode, and the blockage of the active component molecular sieve in the catalyst is difficult to effectively solve, affecting the cracking performance of the catalyst.

Method used

Using an aluminum sol preparation method, by contacting the first aluminum source with acid at 65-90°C, the pH value of the product is adjusted to 2-3, and the second aluminum source is carried out at 60-80°C. Second contact reaction, an aluminum sol with an aluminum-chlorine mass ratio of more than 1.5 was prepared. The Al element is mainly medium and high polymorphism, with a high base degree and acid amount, and is used as a binder for catalytic cracking catalyst.

Benefits of technology

It has achieved high raw material utilization rate, low product price, low impurity content, and is not easy to destroy the Y-type molecular sieve framework. The catalyst has the advantages of low wear index, high mechanical strength and high pore retention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116060044B_ABST
    Figure CN116060044B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of aluminum sol for catalytic cracking catalyst, and discloses an aluminum sol and a preparation method and application thereof. In the aluminum sol, the content of aluminum in terms of Al2O3 is 19-24% by weight, the aluminum-chlorine mass ratio of the aluminum sol is above 1.5, and the aluminum sol has a 27 In the Al NMR spectrum, characteristic peaks exist at chemical shifts of 62.5 and 64.5, and no characteristic peak exists at chemical shift 0. The preparation method comprises: (1) a first contact reaction of a first aluminum source and an acid at a temperature of 65-90°C; (2) adjusting the pH value of the reaction product obtained in step (1) to 2-3; (3) contacting the liquid obtained in step (2) with a second aluminum source for a second contact reaction, wherein the temperature of the second contact reaction is 60-80°C. The production cost is low, and the Al element in the prepared aluminum sol product is mainly in a medium and high polymer state, and basically does not contain monomer aluminum, and the aluminum-chlorine mass ratio is high; as a binder, the prepared catalyst can have the advantages of low wear index, high mechanical strength and high pore retention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of aluminum sol for catalytic cracking catalyst, and in particular to an aluminum sol and a preparation method and application thereof. Background Art

[0002] Fluidized catalytic cracking (FCC) is the most important means of secondary processing of crude oil. At present, the common FCC catalyst preparation process in my country is to prepare the binder, matrix and active matrix into a uniformly mixed slurry and then spray dry it. With the deepening of the heaviness and inferiority of FCC feed, the content of active component molecular sieve in the catalyst has increased to 35-40%, and the corresponding catalyst wear index and sphericity have become a very important issue in the catalyst preparation process. By improving the preparation method of the binder, improving the bonding performance of the binder, and making its particle distribution more uniform, it will be of great significance in reducing the blockage of the molecular sieve pores and improving the activity of the catalyst.

[0003] As an important component of FCC catalyst binder, aluminum sol is a colloidal solution of positively charged hydrated aluminum oxide fine particles uniformly dispersed in water. The properties of aluminum sol can generally be expressed by aluminum content, aluminum-chlorine mass ratio (or molar ratio) or basicity (molar ratio of hydroxide to aluminum). At present, the commonly used preparation methods of aluminum sol include: metal aluminum method, organic alcohol salt hydrolysis method, electrolysis method, inorganic salt raw material method and powder dispersion method, among which the metal aluminum method using metal aluminum and hydrochloric acid to prepare aluminum sol is the main production method in industry.

[0004] US4028216 first introduced in detail the preparation method of metallic aluminum sol. This method has a simple process flow and is easy to operate. However, since aluminum sol is prepared by electrolysis of aluminum hydroxide, the production cost is high and a large amount of electricity is consumed. At the same time, the generation of hydrogen during the preparation process also poses a safety hazard, and the hydrochloric acid used will corrode the equipment.

[0005] CN1445167A discloses a new process for preparing aluminum sol, which comprises: mixing aluminum oxide or / and aluminum hydroxide or / and diaspore as aluminum sources with hydrochloric acid in a molar ratio of Al2O3:HCl=1-1.4:1, and reacting at 80-130°C for 3-40 hours.

[0006] CN1743267A discloses a method for preparing a chlorine-containing aluminum sol, comprising: 1-3 Cl 3-5The aqueous solution of polyaluminium chloride is fully contacted with metallic aluminium to react, and an aluminium sol having an aluminium content of 5-13% by mass and an Al / Cl mass ratio of 0.6-2 is prepared. This method uses polyaluminium chloride to replace part of metallic aluminium to produce aluminium sol, and hydrochloric acid is not used in the production process, which has less corrosion to the equipment, less hydrogen emission, and is safer to operate.

[0007] CN1177653A discloses the use of electrolysis to prepare aluminum sol, synthesizing polyaluminum chloride by electrochemical method with low voltage and high current, using low-cost common anion membrane, reducing the preparation cost of the product, and being more environmentally friendly. However, the electrolysis of water consumes too much energy, has high initial cost (electrodes are required in the repeating unit), may produce chlorine, and has potential safety hazards.

[0008] The hydrolysis of organic alcohol salts can produce sols with high purity, large specific surface area and uniform particle size distribution. This method is suitable for preparing alumina powders with high purity requirements. However, the biggest difficulty in the preparation process is that the raw materials are sensitive to water, the hydrolysis reaction is very rapid, and precipitation is easily formed. In addition, the raw materials are expensive, flammable, toxic, and difficult to preserve, which brings difficulties to industrialization.

[0009] The inorganic salt raw material method uses cheap raw materials and a simple method, which reduces the production cost of aluminum sol, but the purity of the sol is low.

[0010] The powder dispersion method for preparing alumina sol omits the hydrolysis step, the process is simple, and the raw materials are all industrial products, cheap, easy to store, and easy to industrialize. However, the raw materials often contain impurities, and the purity of the prepared aluminum sol is relatively low.

[0011] As the heaviness of crude oil increases, the requirements for the strength and cracking performance of the catalyst are increased. Therefore, improving the binder in the catalyst gelation process, increasing its bonding performance, reducing the blockage of the binder on the molecular sieve structure of the active component in the catalyst, and reducing the influence of the binder on the catalyst activity will be of great significance for the preparation of catalysts that meet the needs of crude oil heavy processing. Summary of the invention

[0012] The object of the present invention is to provide an aluminum sol and a preparation method and application thereof. The preparation method has high raw material utilization rate and simple preparation process. The Al element in the prepared aluminum sol product is mainly in medium and high polymer states, and the aluminum sol product has excellent performance as a binder for catalytic cracking catalysts.

[0013] In order to achieve the above object, the first aspect of the present invention provides an aluminum sol, wherein the aluminum content in terms of Al2O3 is 19-24% by weight, the aluminum chlorine mass ratio of the aluminum sol is above 1.5, and the aluminum sol 27In the Al NMR spectrum, there are characteristic peaks at chemical shifts of 62.5 and 64.5, and no characteristic peak at chemical shift 0.

[0014] A second aspect of the present invention provides a method for preparing aluminum sol, the method comprising the following steps:

[0015] (1) subjecting a first aluminum source to a first contact reaction with an acid at a temperature of 65-90° C.;

[0016] (2) adjusting the pH value of the reaction product obtained in step (1) to 2-3;

[0017] (3) contacting the slurry obtained in step (2) with a second aluminum source to carry out a second contact reaction, wherein the temperature of the second contact reaction is 60-80°C.

[0018] The third aspect of the present invention provides the use of the aluminum sol described in the first aspect or the aluminum sol prepared by the method described in the second aspect in a catalytic cracking catalyst.

[0019] Through the above technical solution, the present invention can achieve the following beneficial effects:

[0020] (1) The raw materials used are cheap and have high utilization rate;

[0021] (2) The obtained aluminum sol product has a high pH value and low impurity content, and is not easy to damage the Y-type molecular sieve framework; the Al element in the aluminum sol is mainly in medium and high polymer states, basically does not contain monomer aluminum, has a high basicity, and has a high acid content;

[0022] (3) The aluminum sol product obtained is used as a binder for preparing a catalytic cracking binder, so that the prepared catalytic cracking catalyst has the advantages of a lower wear index, higher mechanical strength and higher pore retention. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The aluminum sol prepared in Example 1 of the present invention 27 Al NMR spectrum;

[0024] Figure 2 The aluminum sol prepared in Comparative Example 1 of the present invention 27 Al NMR spectrum. DETAILED DESCRIPTION

[0025] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0026] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0027] The first aspect of the present invention provides an aluminum sol, wherein the aluminum content in terms of Al2O3 is 19-24% by weight, the aluminum-chlorine mass ratio of the aluminum sol is above 1.5, and the aluminum sol has a 27 In the Al NMR spectrum, there are characteristic peaks at chemical shifts of 62.5 and 64.5, and no characteristic peak at chemical shift 0.

[0028] The existence form of Al in aluminum sol can be 27 Al NMR spectrum was measured. 27 In the AlNMR spectrum, the δ (chemical shift) of 60-70 corresponds to the characteristic peak of the tetracoordinated aluminum species of the medium and high polymer aluminum, and the δ of 0 corresponds to the characteristic peak of the monomer aluminum. The existence form of the Al element can be determined based on the peak area of ​​the characteristic peak. 27 In the Al NMR spectrum, characteristic peaks exist at δ of 62.5 and 64.5, and no characteristic peak exists at δ of 0, which indicates that the Al element in the aluminum sol provided by the present invention is mainly in medium and high polymer states and substantially does not contain monomer aluminum.

[0029] The Al element is mainly in the form of medium and high polymer states, which means that more than 60% of the Al element exists in the form of medium and high polymer states. The aluminum sol is substantially free of monomer aluminum, which means that the content of Al element in the form of monomer aluminum is less than 10%. By reducing the content of monomer aluminum and increasing the degree of polymerization of aluminum species, the bonding performance of the aluminum sol can be significantly improved.

[0030] According to the present invention, preferably, the aluminum-chlorine mass ratio of the aluminum sol is 1.5-1.8. A higher aluminum-chlorine mass ratio increases the degree of polymerization of aluminum species in the aluminum sol and reduces the content of free chlorine; preferably, the pH of the aluminum sol is above 3.5, and more preferably 3.5-3.7. Within this pH value range, the influence of the aluminum sol on the molecular sieve framework during the preparation of the catalyst can be reduced, thereby making the prepared catalyst have better wear resistance and mechanical strength.

[0031] According to the present invention, preferably, the total acid content of the aluminum sol is 0.4-0.7 mmol / g, and more preferably 0.5-0.6 mmol / g. Aluminum sol has a higher acid content, and using it as a raw material for preparing a catalyst can increase the acidity of the matrix, which is beneficial to improving the heavy oil cracking ability of the catalyst.

[0032] According to the present invention, preferably, the aluminum sol has a specific surface area of ​​105-200m after being calcined at 500°C for 1.5h. 2 / g, pore volume is 0.14-0.2cm 3 / g; preferably, the aluminum sol is calcined at 500°C for 1.5h and then hydrothermally aged at 800°C for 17h to have a specific surface area of ​​60-120m 2 / g, pore volume is 0.18-0.2cm 3 / g. The aluminum sol provided by the present invention still has a good pore structure after aging treatment.

[0033] A second aspect of the present invention provides a method for preparing aluminum sol, the method comprising the following steps:

[0034] (1) subjecting a first aluminum source to a first contact reaction with an acid at a temperature of 65-90° C.;

[0035] (2) adjusting the pH value of the reaction product obtained in step (1) to 2.1-2.8;

[0036] (3) contacting the slurry obtained in step (2) with a second aluminum source to carry out a second contact reaction, wherein the temperature of the second contact reaction is 60-80°C.

[0037] According to the present invention, preferably, the first aluminum source and the second aluminum source are each independently selected from at least one of aluminum hydroxide, aluminum ingot, aluminum flake, aluminum chips, aluminum powder, aluminum chloride, aluminum nitrate, pseudo-boehmite, boehmite, bauxite and aluminum isopropoxide;

[0038] Further preferably, the first aluminum source and the second aluminum source are each independently selected from at least one of aluminum hydroxide, aluminum flakes, aluminum chips, aluminum powder, aluminum isopropoxide and aluminum chloride.

[0039] In the present invention, preferably, the amount of the second aluminum source added is 0.2-0.6 times that of the first aluminum source, and more preferably 0.2-0.5 times.

[0040] According to the present invention, in step (1), from the perspective of improving the uniformity of the contact reaction, preferably, the first contact reaction is carried out under stirring conditions, and the stirring can be carried out in a conventional manner, which is not particularly limited in the present invention, for example, mechanical stirring, magnetic stirring, etc. can be used. Preferably, the stirring speed is 300-500 rpm.

[0041] According to the present invention, in step (1), preferably, the time of the first contact reaction is 6-20 hours, and more preferably 8-20 hours.

[0042] According to the present invention, in step (1), preferably, the mass ratio of the amount of the acid added to the amount of the aluminum element added is 0.6-1.5:1, and more preferably 0.6-1.2:1, wherein the acid is calculated as acid radical, and the aluminum element here refers to total aluminum, that is, the sum of the aluminum elements in the first aluminum source and the second aluminum source.

[0043] In the present invention, the acid can be added all at once in one step, or can be added in steps, preferably in steps, and more preferably in two steps. In the embodiment where the acid is added in two steps, preferably, the amount of acid added in the first step is 40-70% by weight of the total acid amount, stirred for 2-10 hours, and then the remaining acid is added to continue and complete the first contact reaction.

[0044] According to the present invention, in step (1), preferably, the acid is selected from organic acid and / or inorganic acid, and more preferably a mixture of organic acid and inorganic acid. The aluminum sol prepared by this preferred embodiment is used as a raw material for preparing a catalyst, which is more conducive to increasing the pore volume of the matrix. When the acid is an organic acid and an inorganic acid, the ratio of the two is relatively wide, and preferably, the weight ratio of the organic acid: inorganic acid is 0.02-0.2:1.

[0045] Preferably, the inorganic acid is selected from at least one of hydrochloric acid, sulfuric acid and phosphoric acid, more preferably hydrochloric acid; preferably, the organic acid is selected from at least one of formic acid, acetic acid, propionic acid, oxalic acid and citric acid.

[0046] In the present invention, the acid is preferably in the form of an aqueous solution of the acid. In the embodiment where the acid is an inorganic acid, preferably, the concentration of the acid is 5-20% by weight, more preferably 12-18% by weight; in the embodiment where the acid is an organic acid, preferably, the concentration of the acid is 10-12% by weight, more preferably 10-11% by weight; in the embodiment where the acid is a mixture of an organic acid and an inorganic acid, preferably, the concentration of the acid is 5-25% by weight, more preferably 12-20% by weight.

[0047] According to the present invention, in step (2), as long as the pH value of the reaction product obtained in step (1) can be adjusted to 2-3, the range of selection of the added regulator is relatively wide. Preferably, at least one of ammonium salt, inorganic base and organic base is used to adjust the pH value of the reaction product obtained in step (1). The inorganic base is preferably selected from at least one of ammonia water, sodium hydroxide and potassium hydroxide. The organic base is preferably selected from quaternary ammonium salts, and more preferably at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide and tetrapropylammonium hydroxide.

[0048] Preferably, the pH value of the reaction product obtained in step (1) is adjusted to 2.1-2.8, which is beneficial to improving the yield of medium and high polymer aluminum species in the obtained aluminum sol, thereby improving the bonding performance of the aluminum sol.

[0049] According to the present invention, in step (3), the slurry obtained in step (2) is contacted with a second aluminum source to carry out a second contact reaction. From the perspective of improving the uniformity of the contact reaction, preferably, the second contact reaction is carried out under stirring conditions. The stirring method and parameters can be carried out with reference to the method in step (1), which will not be repeated here.

[0050] According to the present invention, in step (3), preferably, the time of the second contact reaction is 5-20 hours, more preferably 5-16 hours.

[0051] According to the present invention, step (3) further comprises cooling the product system obtained by the second contact reaction, and then filtering to obtain the aluminum sol.

[0052] The present invention has no particular limitation on the cooling and filtering, and they can be performed in a conventional manner.

[0053] The third aspect of the present invention provides the use of the aluminum sol described in the first aspect or the aluminum sol prepared by the method described in the second aspect in a catalytic cracking catalyst. The aluminum sol provided by the present invention is used as a binder for a catalytic cracking catalyst, which has the advantages of low wear index, high mechanical strength, and high pore retention.

[0054] The present invention will be described in detail below by way of examples, but the scope of the present invention is not limited thereby. In the following examples and comparative examples,

[0055] The aluminum content and aluminum-chlorine mass ratio in the prepared aluminum sol were determined by the method specified in RIPP34-90 of "Petrochemical Analysis Method (RIPP Test Method)";

[0056] The pH value of aluminum sol was measured using a pH meter (manufacturer: Mettler-Toledo);

[0057] Aluminum sol 27Al NMR spectra were measured using a nuclear magnetic resonance instrument (manufacturer: Bruker, model: AVANCE Ⅲ600WB);

[0058] The pore structure of aluminum sol was measured using a static nitrogen adsorption instrument (manufacturer: Quantachrome Company, model: Autosorb6B);

[0059] The acid content of the aluminum sol was measured using a programmed temperature desorption instrument (manufacturer: Micromeritics, model: AutochemⅡ 2920).

[0060] Example 1

[0061] (1) heating 360 g of a 16 wt % hydrochloric acid solution to 80° C., adding 67 g of an aluminum sheet, maintaining the temperature, and performing a first contact reaction at a stirring rate of 500 rpm for 18 h;

[0062] (2) cooling the reaction product obtained in step (1) to 65° C., slowly dropping ammonia water into the reaction product to adjust the pH value of the solution to 2.6;

[0063] (3) Slowly add 17 g of aluminum chips to the liquid obtained in step (2), control the temperature at 75° C., continue stirring, and carry out the second contact reaction for 10 hours. After the reaction is completed, wait for the product to cool to ambient temperature (25° C., the same below), filter, and obtain aluminum sol P1 with a concentration of 23.5% by weight (calculated as Al2O3).

[0064] The pH value of P1 is 3.5, the aluminum-chlorine mass ratio is 1.52, and the total acid content is 0.56 mmol / g. The BET specific surface area and pore volume of P1 after calcination at 500℃ for 1.5h and hydrothermal aging at 800℃ for 17h are shown in Table 1.

[0065] P1 27 Al NMR spectrum Figure 1 As shown, from Figure 1 It can be seen that there are characteristic peaks of tetracoordinate aluminum species of medium-polymerized aluminum at δ of 62.5 and 64.5, and a characteristic peak of tetracoordinate aluminum species of high-polymerized aluminum at δ of 70 (partially overlapping with the characteristic peak at δ of 65 in the figure), and there is no characteristic peak of monomeric aluminum at δ of 0. It can be seen that the Al element in P1 mainly exists in medium and high-polymerized forms, and basically does not contain monomeric aluminum.

[0066] Comparative Example 1

[0067] 360 g of a 16 wt % hydrochloric acid solution was heated to 80° C., 67 g of aluminum flakes were added, the temperature was maintained, and the contact reaction was carried out at a stirring rate of 500 rpm for 20 h. After the reaction was completed, the product was cooled to ambient temperature (25° C., the same below), filtered, and an aluminum sol D1 with a concentration of 20 wt % (calculated as Al2O3) was obtained.

[0068] The pH value of D1 is 2.5, the aluminum-chlorine mass ratio is 1.2, and the total acid content is 0.33 mmol / g. The BET specific surface area and pore volume of D1 after calcination at 500℃ for 1.5h and hydrothermal aging at 800℃ for 17h are shown in Table 1.

[0069] D1 27 Al NMR spectrum Figure 2 As shown, from Figure 2 It can be seen that there is a characteristic peak of tetracoordinated aluminum species of mesopolymerized aluminum at δ of 64.5, and a characteristic peak of monomeric aluminum at δ of 0.

[0070] It can be seen from Table 1 that after calcination at 500℃ for 1.5h and hydrothermal aging at 800℃ for 17h, the BET specific surface area and pore volume of aluminum sol P1 are higher than those of aluminum sol D1. P1 can still maintain a relatively high pore structure after hydrothermal aging at 800℃ for 17h.

[0071] Example 2

[0072] The method of Example 1 is followed, except that in step (1), 360 g of 16 wt% hydrochloric acid is added in two steps, specifically, 180 g of 16 wt% hydrochloric acid solution is first heated to 80°C, 67 g of aluminum flakes are added, and a first contact reaction is carried out at a stirring rate of 500 rpm for 10 h, and then 180 g of 16 wt% hydrochloric acid solution is continuously added, and the first contact reaction is continued for 10 h. Other conditions are the same as those of Example 1, and an aluminum sol P2 with a concentration of 23.2 wt% (in terms of Al2O3) is obtained.

[0073] The pH value of P2 is 3.5, the aluminum-chlorine mass ratio is 1.54, and the total acid content is 0.57mmol / g. P2 has similar 27 AlNMR spectrum.

[0074] Example 3

[0075] The method of Example 1 is followed, except that in step (2), tetrapropylammonium hydroxide solution is slowly added dropwise to adjust the pH value of the liquid to 2.6. Other conditions are the same as those of Example 1, and an aluminum sol P3 with a concentration of 23 wt% (in terms of Al2O3) is obtained.

[0076] The pH value of P3 is 3.5, the aluminum-chlorine mass ratio is 1.52, and the total acid content is 0.52mmol / g. P3 has similar 27 AlNMR spectrum.

[0077] Example 4

[0078] The method of Example 1 is followed, except that in step (3), 17 g of aluminum flakes are added to the slurry obtained in step (2), and the time of the second contact reaction is controlled to be 16 h. Other conditions are the same as those of Example 1, and an aluminum sol P4 with a concentration of 23.2 wt% (calculated as Al2O3) is obtained.

[0079] The pH value of P4 is 3.5, the aluminum-chlorine mass ratio is 1.52, and the total acid content is 0.54mmol / g. P4 has similar 27 AlNMR spectrum.

[0080] Example 5

[0081] The method of Example 1 is followed, except that in step (2), a mixture of ammonium chloride and ammonia water is slowly dripped to adjust the pH value of the feed solution to 2.6. Other conditions are the same as those of Example 1, and an aluminum sol P5 with a concentration of 23.8 wt% (in terms of Al2O3) is obtained.

[0082] The pH value of P5 is 3.5, the aluminum-chlorine mass ratio is 1.5, and the total acid content is 0.5mmol / g. P5 has similar 27 AlNMR spectrum.

[0083] Example 6

[0084] (1) heating a mixed solution of 350 g of 16 wt % hydrochloric acid and 55 g of 5 wt % acetic acid to 80° C., adding 67 g of aluminum chips, maintaining the temperature, and performing a first contact reaction at a stirring rate of 500 rpm for 15 h;

[0085] (2) cooling the reaction product obtained in step (1) to 60° C., slowly dropping ammonia water into the reaction product to adjust the pH value of the solution to 2.3;

[0086] (3) 17 g of aluminum chips were added to the liquid obtained in step (2), and the temperature was controlled at 75° C., and stirring was continued to carry out the second contact reaction for 10 hours. After the reaction was completed, the product was cooled to ambient temperature (25° C., the same below), filtered, and an aluminum sol P6 with a concentration of 23% by weight (calculated as Al2O3) was obtained.

[0087] The pH value of P6 is 3.5, the aluminum-chlorine mass ratio is 1.56, and the total acid content is 0.58mmol / g. P6 has similar 27 AlNMR spectrum.

[0088] Table 1

[0089]

[0090] Test Case

[0091] Alumina sols P1-P6 and D1 prepared in Examples 1-6 and Comparative Example 1 were used as binders to prepare catalytic cracking catalysts, and the prepared catalysts were subjected to a wear index test. The preparation method of the catalytic cracking catalyst comprises:

[0092] Kaolin and water were slurried, and then acidified pseudo-boehmite was added (pseudo-boehmite was mixed with water, and then hydrochloric acid was added thereto under stirring to acidify until it was in a peptized state), and stirred to obtain slurry A; HRY-1 molecular sieve was slurried with water to obtain molecular sieve slurry; slurry A and molecular sieve slurry were added to the aluminum sol prepared in the above embodiment and comparative example respectively, and stirred for 30 minutes to obtain catalyst slurry (solid content was 27 weight %), in which, based on the dry weight of the catalyst slurry, the content of HRY-1 molecular sieve was 35 weight %, the content of kaolin was 35 weight %, the content of aluminum sol (calculated as Al2O3) was 13 weight %, and the content of pseudo-boehmite (calculated as Al2O3) was 17 weight %. The catalyst slurry was spray dried, and the obtained catalyst microspheres were calcined at 550° C. for 1.5 hours to obtain a catalytic cracking catalyst.

[0093] Wear index test

[0094] According to the method specified in RIPP29-90 of "Petrochemical Analysis Method (RIPP Test Method)", the 4h wear index of the catalytic cracking catalyst prepared above was evaluated. The results are shown in Table 2.

[0095] Table 2

[0096] catalyst 4h wear and tear rate / % Wear index Catalyst prepared by P1 3.56 0.89 Catalyst prepared by P2 3.24 0.81 Catalyst prepared by P3 2.84 0.71 Catalyst prepared by P4 3.4 0.85 Catalyst prepared by P5 3.6 0.9 Catalyst prepared by P6 1.8 0.45 Catalyst prepared by D1 7.2 1.8

[0097] As can be seen from Table 2, the aluminum sol prepared by the method provided by the present invention has better bonding performance than conventional industrial aluminum sol. When used as a binder for preparing catalytic cracking catalysts, the prepared catalysts can have a lower wear index and thus obtain higher mechanical strength. It can be seen from Example 1 and Comparative Example 1 that the aluminum sol provided by the present application also has a higher pore retention.

[0098] The aluminum sol preparation method provided by the present invention has low raw material price, neutralizes more free chlorine, so the raw material utilization rate is high, the whole preparation process conditions are mild, and high-quality aluminum sol products can be produced. The pH value of the prepared aluminum sol product is high, the Al element therein is mainly in medium and high polymer states, basically does not contain monomer aluminum, has a high aluminum-chlorine mass ratio, and has strong bonding performance. After the catalyst is prepared, compared with the catalyst prepared by conventional aluminum sol, the catalyst has a low wear index, a high mechanical strength and a high pore retention under the same composition and colloidal solid content.

[0099] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. An aluminum sol, wherein the aluminum content in terms of Al2O3 is 19-24% by weight, the aluminum-chlorine mass ratio of the aluminum sol is above 1.5, and the aluminum sol 27 In the Al NMR spectrum, there are characteristic peaks at chemical shifts 62.5 and 64.5, but no characteristic peak at chemical shift 0; The pH of the aluminum sol is above 3.5; the total acid content of the aluminum sol is 0.4-0.7 mmol / g.

2. The aluminum sol according to claim 1, wherein The aluminum sol has an aluminum-chlorine mass ratio of 1.5-1.8; And / or, the pH of the aluminum sol is 3.5-3.

7.

3. The aluminum sol according to claim 1 or 2, wherein The total acid content of the aluminum sol is 0.5-0.6 mmol / g.

4. The aluminum sol according to claim 1 or 2, wherein After the aluminum sol is calcined at 500°C for 1.5 hours, the specific surface area is 105-200m 2 / g, pore volume is 0.14-0.2cm 3 / g; And / or, the aluminum sol is calcined at 500°C for 1.5 hours and then hydrothermally aged at 800°C for 17 hours, and the specific surface area is 60-120m 2 / g, pore volume is 0.18-0.2cm 3 / g.

5. The aluminum sol according to claim 3, wherein After the aluminum sol is calcined at 500°C for 1.5 hours, the specific surface area is 105-200m 2 / g, pore volume is 0.14-0.2cm 3 / g; And / or, the aluminum sol is calcined at 500°C for 1.5 hours and then hydrothermally aged at 800°C for 17 hours, and the specific surface area is 60-120m 2 / g, pore volume is 0.18-0.2cm 3 / g.

6. A method for preparing the aluminum sol according to any one of claims 1 to 5, the method comprising the following steps: (1) subjecting a first aluminum source to a first contact reaction with an acid at a temperature of 65-90° C.; (2) adjusting the pH value of the reaction product obtained in step (1) to 2-3; (3) The slurry obtained in step (2) is contacted with a second aluminum source to carry out a second contact reaction, wherein the temperature of the second contact reaction is 60-80° C., to obtain an aluminum sol.

7. The preparation method according to claim 6, wherein: The first aluminum source and the second aluminum source are each independently selected from at least one of aluminum hydroxide, aluminum ingot, aluminum flake, aluminum chips, aluminum powder, aluminum chloride, aluminum nitrate, pseudo-boehmite, boehmite, bauxite, and aluminum isopropoxide; And / or, the added amount of the second aluminum source is 0.2-0.6 times that of the first aluminum source.

8. The preparation method according to claim 7, wherein: The first aluminum source and the second aluminum source are each independently selected from at least one of aluminum hydroxide, aluminum flakes, aluminum chips, aluminum powder, aluminum isopropoxide, and aluminum chloride; And / or, the added amount of the second aluminum source is 0.2-0.5 times that of the first aluminum source.

9. The preparation method according to any one of claims 6 to 8, wherein: The first contact reaction is carried out under stirring conditions, and the stirring speed is 300-500 rpm; And / or, the first contact reaction time is 6-20h; And / or, the mass ratio of the amount of the acid added to the amount of the aluminum element added is 0.6-1.5:1, wherein the acid is calculated as acid radical; And / or, the acid is added in one step or in stages.

10. The preparation method according to claim 9, wherein: The first contact reaction time is 8-20h; And / or, the mass ratio of the amount of the acid added to the amount of the aluminum element added is 0.6-1.2:1, wherein the acid is calculated as acid radical; And / or, the acid is added in two steps.

11. The preparation method according to claim 10, wherein: In the first step, the amount of acid added is 40-70% by weight of the total acid amount, stirred for 2-10 hours, and then the remaining acid is added.

12. The preparation method according to any one of claims 6 to 8, wherein: The acid is selected from organic acids and / or inorganic acids.

13. The preparation method according to claim 12, wherein: The acid is an organic acid and an inorganic acid.

14. The preparation method according to claim 12, wherein: The inorganic acid is selected from at least one of hydrochloric acid, sulfuric acid and phosphoric acid; And / or, the organic acid is selected from at least one of formic acid, acetic acid, propionic acid, oxalic acid and citric acid.

15. The preparation method according to claim 14, wherein: The inorganic acid is hydrochloric acid.

16. The preparation method according to claim 13, wherein: The inorganic acid is selected from at least one of hydrochloric acid, sulfuric acid and phosphoric acid; And / or, the organic acid is selected from at least one of formic acid, acetic acid, propionic acid, oxalic acid and citric acid.

17. The preparation method according to claim 16, wherein: The inorganic acid is hydrochloric acid.

18. The preparation method according to any one of claims 6 to 8, wherein: In step (2), the pH value of the reaction product obtained in step (1) is adjusted to 2.1-2.8; and / or, in step (2), at least one of an ammonium salt, an inorganic base and an organic base is used to adjust the pH value of the reaction product obtained in step (1); And / or, in step (3), the second contact reaction time is 5-20 hours.

19. The preparation method according to claim 18, wherein: In step (3), the second contact reaction time is 5-16 hours.

20. Use of the aluminum sol according to any one of claims 1 to 5 in a catalytic cracking catalyst.