Hydrofining catalyst grading method and hydrofining method

By adopting a specific structure of the first and second hydrogenation catalyst gradations in the hydrodesulfurization catalyst, the problem of insufficient activity and stability of the existing catalysts in high and low temperature reaction environments is solved, and the diesel hydrodesulfurization reaction is realized. Efficient operation meets higher standards of clean diesel production needs.

CN116060051BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111271614.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-10-15
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

Existing hydrodesulfurization catalyst systems have deficiencies in activity and stability and cannot meet the long-term production requirements of higher standards of clean diesel, especially in high- and low-temperature reaction environments.

Method used

A hydrorefining catalyst grading method is adopted, by sequentially loading the first hydrogenation catalyst and the second hydrogenation catalyst along the flow direction. The first hydrogenation catalyst contains Group VIII metal, Group VIB metal and alumina, with a pore size distribution of 2 -6nm and 8-20nm Bimodal type, the second hydrogenation catalyst contains Group VIII and Group VIB metals supported on alumina. The pore size is unimodal in the range of 8-20nm. The volume ratio of the two is 1:4-4:1, ensuring that the catalyst Maintain high activity and stability under different reaction conditions.

Benefits of technology

It achieves smooth and efficient operation of the hydrodesulfurization reaction under high and low temperature conditions, significantly improves the activity and stability of the catalyst, and meets more stringent clean diesel production standards.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of hydrofining, and discloses a hydrofining catalyst grading method and a hydrofining method. The hydrofining catalyst grading method includes: a first hydrogenation catalyst and a second hydrogenation catalyst sequentially loaded along the logistics direction; the loading volume ratio of the first hydrogenation catalyst and the second hydrogenation catalyst is 1:4-4:1; the first hydrogenation catalyst comprises at least one Group VIII metal element, at least one Group VIB metal element and alumina, and the pore size of the first hydrogenation catalyst presents a bimodal pore distribution within the range of 2-6nm and 8-20nm; the second hydrogenation catalyst comprises alumina and Group VIII metal elements and Group VIB metal elements loaded on alumina, and the pore size of the second hydrogenation catalyst presents a unimodal pore distribution within the range of 8-20nm. The grading method uses catalysts in combination, and the hydrodesulfurization reaction system can be applied to both high-temperature reactions and low-temperature reactions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrofining, and in particular to a hydrofining catalyst grading method and a hydrofining method. Background Art

[0002] With the continuous tightening of environmental protection regulations, the production of clean fuels has received more attention from the society, and refineries need to provide clean fuels that meet the latest environmental protection regulations in a long period of time and stably. The latest diesel quality indicators require that the sulfur content and polycyclic aromatic hydrocarbons be reduced to 10 mg / kg and 7% respectively, which leads to an increase in the severity of the diesel hydrotreating unit, accelerates the deactivation of the catalyst, compresses the temperature operating space of the unit, and greatly shortens the operation cycle. The industrial diesel hydrotreating unit is an adiabatic reactor, and the temperature difference in the axial direction of the reactor is large, resulting in significantly different reaction chemical environments for hydrodesulfurization and hydrodearomatization. Therefore, the diesel hydrodesulfurization catalyst should be adapted to the reaction environment at different stages, and the development of catalyst grading technology has become an important technical research and development direction. The patent application with application number 201210409647.0 discloses a method for hydrodesulfurization of distillate oil, which uses at least two catalysts for grading, the catalyst has Mo and Ni and / or Co as active metal components, P as an additive, and contains alkali metal salts of heteropoly acids, and the content of alkali metal salts of heteropoly acids in the graded catalyst increases successively along the flow direction of the fluid.

[0003] The patent application with application number 201010221051.9 discloses a diesel hydrodesulfurization method with catalyst grading loading, wherein two or more catalyst beds are provided, and a mixed catalyst bed is composed of Mo-Co type catalyst and Mo-Ni type catalyst, and the proportion of Mo-Ni catalyst in the mixed bed gradually increases. Patent 201110192780.0 divides the reactor into four reaction zones, which are respectively loaded with the first type of catalyst, a mixture of the first type of catalyst and the second type of catalyst, the second type of catalyst and the first type of catalyst, wherein the first type of catalyst is Mo-Co catalyst, and the second type of catalyst is W-Mo-Ni catalyst or W-Ni. This process treats high-sulfur, high-nitrogen low-quality diesel by grading different catalysts.

[0004] At present, the hydrodesulfurization catalyst system still has certain deficiencies in activity and stability, and cannot fully meet the needs of long-term production of higher standard clean diesel. In view of the deficiencies of the current technology, the present invention discloses a high-performance hydrorefining catalyst grading system with high activity and stability. Summary of the invention

[0005] The purpose of the present invention is to overcome the problem of insufficient activity and stability of the hydrodesulfurization catalyst system in the prior art, and to provide a hydrorefining catalyst grading method and a hydrorefining method. The grading method combines the good activity and stability of a first hydrogenation catalyst and a second hydrogenation catalyst, so that the hydrodesulfurization reaction system can be suitable for both high-temperature reactions and low-temperature reactions, thereby ensuring the smooth and efficient operation of the hydrodesulfurization system.

[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a method for grading a hydrorefining catalyst, which comprises: a first hydrogenation catalyst and a second hydrogenation catalyst are sequentially loaded along a logistics direction; the loading volume ratio of the first hydrogenation catalyst and the second hydrogenation catalyst is 1:4-4:1; the first hydrogenation catalyst comprises at least one metal element of Group VIII, at least one metal element of Group VIB and alumina, and the pore size of the first hydrogenation catalyst presents a bimodal pore distribution in the range of 2-6nm and 8-20nm; the second hydrogenation catalyst comprises alumina and the metal element of Group VIII and the metal element of Group VIB loaded on the alumina, and the pore size of the second hydrogenation catalyst presents a unimodal pore distribution in the range of 8-20nm.

[0007] Preferably, the packing volume ratio of the first hydrogenation catalyst to the second hydrogenation catalyst is 1:3-3:1.

[0008] Preferably, the first hydrogenation catalyst composition is (Xi ai )·(Yi bi )·(Zi ci )·Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of the carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of the carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of the carrier P2O5, Sup refers to the carrier, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.4-0.9nm, preferably 0.5-0.8nm, ρ Xi , Yi , Zi are the densities of VIB group metal oxides, VIII group metal oxides and P2O5, SA sup is the specific surface area of ​​the carrier.

[0009] Preferably, the second hydrogenation catalyst composition is (Xi ai )·(Yi bi )·(Zi ci)·Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of carrier P2O5, Sup refers to the carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.18-0.39nm, preferably 0.25-0.38nm, ρ Xi , Yi , Zi are the densities of VIB group metal oxides, VIII group metal oxides and P2O5, SA sup is the specific surface area of ​​the carrier.

[0010] The second aspect of the present invention provides a hydrorefining method, which comprises: under hydrorefining conditions, injecting a feedstock to be hydrorefined into a hydrorefining device for reaction, wherein the catalyst in the hydrorefining device is loaded according to the grading method described in the first aspect.

[0011] Through the above technical scheme, the first hydrogenation catalyst and the second hydrogenation catalyst with a specific structure and composition are loaded according to a specific loading volume ratio, so that the two can cooperate with each other and be applied to the clean production of diesel. They can not only realize the hydrodesulfurization reaction under low temperature conditions, but also complete the hydrodesulfurization reaction under high temperature conditions. Both catalysts have good activity and stability and have excellent industrial value. DETAILED DESCRIPTION

[0012] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0013] The first aspect of the present invention provides a method for grading a hydrorefining catalyst, which comprises: a first hydrogenation catalyst and a second hydrogenation catalyst are sequentially loaded along a logistics direction; the loading volume ratio of the first hydrogenation catalyst and the second hydrogenation catalyst is 1:4-4:1; the first hydrogenation catalyst comprises at least one metal element of Group VIII, at least one metal element of Group VIB and alumina, and the pore size of the first hydrogenation catalyst presents a bimodal pore distribution in the range of 2-6nm and 8-20nm; the second hydrogenation catalyst comprises alumina and the metal element of Group VIII and the metal element of Group VIB loaded on the alumina, and the pore size of the second hydrogenation catalyst presents a unimodal pore distribution in the range of 8-20nm.

[0014] In the present invention, the pore size of the first hydrogenation catalyst presents a bimodal pore distribution in the range of 2-6 nm and 8-20 nm, which means that the pore size distribution of the first hydrogenation catalyst has two peaks in the pore size range of 2-6 nm and 8-20 nm. Generally, the carrier also has a certain number of pore size distributions in the range of 2-6 nm, but this part of the pores of the carrier does not have a peak, and no bimodal pores are formed.

[0015] In the present invention, the second hydrogenation catalyst presenting a unimodal pore size distribution in the range of 8-20 nm means that the pore size distribution of the second hydrogenation catalyst presents a peak in the range of 8-20 nm.

[0016] In the present invention, the first hydrogenation catalyst contains metal elements of Group VIII and metal elements of Group VIB loaded on alumina, so that the pores of the first hydrogenation catalyst present a bimodal pore distribution, with a portion of the pores concentrated at the position where the pore diameter is concentrated in the carrier, and the other portion concentrated at 2-6 nm. Due to the loading of active metal components, pores at 2-6 nm are generated, and this bimodal pore structure can meet the requirements of the reaction molecules to diffuse to the active center, and can load sufficient active metal components, so that the desulfurization performance of the hydrorefining catalyst is greatly improved.

[0017] In the present invention, by controlling the composition and structure of the second hydrogenation catalyst, it is suitable for the hydrodesulfurization reaction under high temperature conditions. The second hydrogenation catalyst has good activity and stability at high temperatures, can exert excellent performance at high temperatures, and will be more suitable for the high-temperature reaction zone of the industrial adiabatic reaction environment.

[0018] In the present invention, the first hydrogenation catalyst and the second hydrogenation catalyst with a specific structure and composition are loaded according to a specific loading volume ratio, so that the two can cooperate with each other and exert a synergistic effect. When applied to clean diesel production, the first hydrogenation catalyst and the second hydrogenation catalyst with a specific structure and composition are loaded according to a specific loading volume ratio, so that the two can cooperate with each other and exert a synergistic effect. When applied to clean diesel production, the first hydrogenation catalyst and the second hydrogenation catalyst can realize a hydrogenation desulfurization reaction under low temperature conditions and complete a hydrogenation desulfurization reaction under high temperature conditions, thereby improving the reaction efficiency and ensuring that the reaction proceeds smoothly and continuously, and the invention has excellent industrial value.

[0019] In a preferred case, the loading volume ratio of the first hydrogenation catalyst to the second hydrogenation catalyst is 1: 3-3: 1. This preferred embodiment can give full play to the advantages of the catalysts in the upper and lower beds, better promote the synergistic effect of the first hydrogenation catalyst and the second hydrogenation catalyst, and keep the catalysts at a high desulfurization and stability.

[0020] In a preferred embodiment, the equivalent diameters of the first hydrogenation catalyst and the second hydrogenation catalyst are independently 0.5-1.8 mm, preferably 0.8-1.6 mm.

[0021] In the present invention, there is no specific limitation on the shapes of the first hydrogenation catalyst and the second hydrogenation catalyst, and the two may be the same or different. Preferably, the shapes of the first hydrogenation catalyst and the second hydrogenation catalyst are each independently butterfly-shaped, cylindrical, three-leaf clover, four-leaf clover, honeycomb-shaped or other irregular shapes, and more preferably butterfly-shaped.

[0022] In the present invention, the first hydrogenation catalyst has specific physicochemical parameters, so that the first hydrogenation catalyst is suitable for hydrodesulfurization reaction. Preferably, the pore volume of the first hydrogenation catalyst with a pore size distribution of 2-6 nm accounts for 8-15% of the total pore volume of the catalyst, preferably 9-12%. The advantage of adopting this preferred embodiment is that the effect of the active metal components in the smaller pores and the larger pores can be fully exerted, thereby improving the reaction efficiency of the first hydrogenation catalyst for different sulfur-containing compounds.

[0023] In a preferred embodiment, the specific surface area of ​​the first hydrogenation catalyst is 130-170 m 2 / g.

[0024] In a preferred embodiment, the pore volume of the first hydrogenation catalyst is 0.25-0.4 cm 3 / g, more preferably 0.28-0.4cm 3 / g.

[0025] In a preferred embodiment, the average pore size of the first hydrogenation catalyst is 8-10 nm.

[0026] In the present invention, preferably, the first hydrogenation catalyst further contains phosphorus.

[0027] In a preferred embodiment, the first hydrogenation catalyst composition is (Xi ai )·(Yi bi )·(Zi ci)·Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of the carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of the carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of the carrier P2O5, Sup refers to the carrier, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.4-0.9nm, preferably 0.5-0.8nm, ρ Xi , Yi , Zi are the densities of VIB group metal oxides, VIII group metal oxides and P2O5, SA sup is the specific surface area of ​​the carrier.

[0028] In the present invention, ρMoO3, ρWO3, ρNiO, ρCoO, and ρP2O5 are 4.69 g / cm 3 、7.16g / cm 3 、6.67g / cm 3 、6.45g / cm 3 and 2.39 g / cm 3 calculate.

[0029] In the present invention, the Group VIII metal element includes but is not limited to at least one of Fe, Co, Ni, Ru, Pt and Pd, preferably Co and / or Ni.

[0030] In a preferred embodiment, the VIB Group metal element includes but is not limited to at least one of Cr, Mo and W, preferably Mo and / or W.

[0031] In the present invention, there is no specific limitation on the amount of P2O5 and the metal oxide of Group VIB. Preferably, the molar ratio of Zi / Xi in the first hydrogenation catalyst is 0.05-0.3, and more preferably 0.08-0.2. The advantage of adopting this preferred embodiment is that the metal combination method is adopted, so that each metal component can better play a synergistic effect with each other, thereby optimizing the activity of the first hydrogenation catalyst.

[0032] In the present invention, the second hydrogenation catalyst also has specific physicochemical parameters, and the second hydrogenation catalyst is excellently suitable for hydrodesulfurization reaction under high temperature conditions. Preferably, the pore volume of the second hydrogenation catalyst with a pore size distribution of 8-20 nm accounts for 50-80% of the total pore volume of the catalyst, preferably 60-75%.

[0033] In a preferred embodiment, the specific surface area of ​​the second hydrogenation catalyst is 185-210m 2 / g.

[0034] In a preferred embodiment, the pore volume of the second hydrogenation catalyst is 0.4-0.6 cm 3 / g, more preferably 0.4-0.5cm 3 / g.

[0035] In a preferred embodiment, the average pore size of the second hydrogenation catalyst is 6-18 nm, more preferably 8-12 nm.

[0036] In the present invention, the second hydrogenation catalyst also contains phosphorus.

[0037] In the present invention, a second hydrogenation catalyst having the above-mentioned physicochemical parameters is provided. Preferably, the second hydrogenation catalyst composition is as follows: ai )·(Yi bi )·(Zi ci )·Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of carrier P2O5, Sup refers to the carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.18-0.39nm, preferably 0.25-0.38nm, ρ Xi , Yi , Zi are the densities of VIB group metal oxides, VIII group metal oxides and P2O5, SA sup is the specific surface area of ​​the carrier. By using the above expression to define the composition of the second hydrogenation catalyst, the pores of the catalyst remain at a relatively large level after the active metal components of the catalyst are loaded on the alumina carrier, forming an unobstructed diffusion channel, slowing down the carbon deposition of the catalyst, and promoting the stability of the hydrogenation catalyst at high temperature, so that the second hydrogenation catalyst is particularly suitable for hydrodesulfurization reaction under high temperature conditions.

[0038] In the present invention, the types of the VIB group metal element and the VIII group metal element in the second hydrogenation catalyst are the same as those of the first hydrogenation catalyst, and will not be elaborated herein.

[0039] In the present invention, there is no specific limitation on the amount of P2O5 and the metal oxide of Group VIB in the second hydrogenation catalyst, and those skilled in the art can select them according to specific performance requirements. Preferably, the molar ratio of Zi / Xi in the second hydrogenation catalyst is 0.1-0.35:1, and more preferably 0.2-0.35:1. The advantage of adopting this preferred embodiment is to promote the dissolution of the active metal component, maintain a moderate amount of phosphate, and improve the dispersion ability of the active metal component.

[0040] In the present invention, the specific surface area, pore volume, average pore diameter and pore distribution of the first hydrogenation catalyst and the second hydrogenation catalyst are measured after calcination at 400° C. for 3 hours.

[0041] In the present invention, the specific surface area, pore volume, average pore diameter and pore distribution of the first hydrogenation catalyst and the second hydrogenation catalyst are measured by low temperature nitrogen adsorption method (BET) (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). Among them, the pore volume of 2-100 nm is calculated according to the results of BET.

[0042] In the present invention, unless otherwise specified, the 2-6nm pores refer to pores with a pore diameter greater than or equal to 2nm and less than 6nm, the 2-4nm pores refer to pores with a pore diameter greater than or equal to 2nm and less than 4nm, the 4-6nm pores refer to pores with a pore diameter greater than or equal to 4nm and less than 6nm, and the 8-20nm pores refer to pores with a pore diameter greater than or equal to 8nm and less than 20nm.

[0043] In the present invention, there is no particular limitation on the carriers required for the first hydrogenation catalyst and the second hydrogenation catalyst, and conventional carriers in the art are applicable to the present invention. Preferably, the first hydrogenation catalyst and the second hydrogenation catalyst use the same alumina, and the water absorption rate of the alumina used is greater than 0.9 mL / g, more preferably 0.9-1.1 mL / g, and the specific surface area is greater than 260 m 2 / g, more preferably 270-280m 2 / g, the average pore size is greater than 8nm, more preferably 10-12nm, and the pore distribution morphology is a unimodal pore distribution.

[0044] In a preferred embodiment, in the alumina, the volume of pores with a pore size distribution of 2-6 nm accounts for no more than 10% of the total pore volume of the alumina, preferably no more than 8%, and more preferably 5-8%.

[0045] In a preferred embodiment, in the alumina, the volume of pores with pore diameter distribution in the range of 2-4 nm accounts for no more than 4%, preferably no more than 2% of the total pore volume of the alumina.

[0046] The advantages of using the above-mentioned alumina carrier are to provide a larger specific surface area, promote the dispersion of the active phase; provide a larger reaction channel, promote better contact of the reaction molecules with the active center at high temperature; reduce the smaller pore size, promote uniform pore size, reduce the formation of carbon deposits, promote volumetric carbon capacity, and improve the stability of the first hydrogenation catalyst and the second hydrogenation catalyst.

[0047] In the present invention, in order to further improve the hydrodesulfurization performance of the first hydrogenation catalyst, preferably, the atomic concentration of the VIB group metal element on the carrier surface in the first hydrogenation catalyst is 5-13 atom / nm 2 , preferably 5-11atom / nm 2 .

[0048] In the present invention, the second hydrogenation catalyst is also limited so that the performance of the second hydrogenation catalyst is improved. Preferably, the atomic concentration of the metal element of Group VIB on the carrier surface in the second hydrogenation catalyst is 2-6 atom / nm 2 , preferably 3-4.5atom / nm 2 .

[0049] In the present invention, the atomic concentration of the VIB group metal element on the surface of the carrier in the first hydrogenation catalyst and the second hydrogenation catalyst refers to the average atomic concentration of the VIB group metal element on the surface of the carrier, which is obtained by measuring the metal loading and the specific surface area of ​​the carrier and then calculating. Specifically, it is obtained by the following calculation formula: atomic concentration = (a / M Xi )×N A / (1×SA sup ), where N A is Avogadro's constant, ai is the mass relative to 1 gram of carrier Xi, M Xi is the molecular weight of Xi, SA sup The advantage of using the atomic concentration within this range is that a moderate number of active centers are formed, which on the one hand meets the needs of the reaction, and on the other hand leaves enough space to achieve the purpose of promoting diffusion and reducing carbon deposition.

[0050] In a preferred embodiment, the atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the first hydrogenation catalyst is 0.05-0.35, preferably 0.1-0.3.

[0051] In a preferred embodiment, the atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the second hydrogenation catalyst is 0.2-0.4, preferably 0.2-0.35.

[0052] According to the present invention, preferably, the first hydrogenation catalyst and the second hydrogenation catalyst further independently comprise an organic alcohol compound and / or a carboxylic acid compound.

[0053] According to the present invention, the organic alcohol compound can be at least one of a monohydric alcohol, a dihydric alcohol and a polyhydric alcohol. In a preferred embodiment, the organic alcohol compound is selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, amyl alcohol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol and trimethylolethane, preferably at least one of glycerol, propanol and ethylene glycol.

[0054] In a preferred embodiment, the carboxylic acid compound is selected from one or more of formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid and tartaric acid, preferably at least one of formic acid, citric acid and acetic acid.

[0055] In a particularly preferred case, the first hydrogenation catalyst and the second hydrogenation catalyst each independently contain one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol, trimethylolethane and / or formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid, tartaric acid.

[0056] In a preferred embodiment, in the first hydrogenation catalyst and the second hydrogenation catalyst, the molar ratio of the organic alcohol compound and / or the carboxylic acid compound to the Group VIII metal element is independently 1 to 6, preferably 2 to 5. The advantages of adopting this preferred embodiment are to promote the Group VIII metal element to have a higher dispersion ability, weaken the interaction between the support and the metal, and promote the generation of more active phases.

[0057] In the present invention, there is no specific limitation on the preparation methods of the first hydrogenation catalyst and the second hydrogenation catalyst. Preferably, the preparation methods of the first hydrogenation catalyst and the second hydrogenation catalyst each independently comprise: introducing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and optionally an organic alcohol compound and / or a carboxylic acid compound into alumina by an impregnation method, and then drying.

[0058] According to the present invention, the "optionally containing organic alcohol compounds and / or carboxylic acid compounds" means that organic alcohol compounds and / or carboxylic acid compounds may or may not be introduced into alumina, but introduction is preferred.

[0059] In the present invention, the metal element species in the VIB group metal oxide and the VIII group metal oxide are provided by a precursor containing the above metal elements. Preferably, the VIB group metal precursor is selected from at least one of ammonium heptamolybdate, ammonium molybdate, ammonium phosphomolybdate, molybdenum oxide, ammonium metatungstate, ethylammonium metatungstate and tungsten oxide.

[0060] In a preferred embodiment, the Group VIII metal precursor is at least one selected from cobalt nitrate, basic cobalt carbonate, cobalt acetate, cobalt oxide, nickel nitrate, basic nickel carbonate, nickel acetate and nickel oxide.

[0061] In a particularly preferred embodiment, the VIB Group metal and VIII Group metal precursor is selected from at least one of ammonium heptamolybdate, ammonium molybdate, ammonium phosphomolybdate, molybdenum oxide, ammonium metatungstate, ethylammonium metatungstate, tungsten oxide, cobalt nitrate, basic cobalt carbonate, cobalt acetate, cobalt oxide, nickel nitrate, basic nickel carbonate, nickel acetate and nickel oxide.

[0062] In the present invention, P2O5 is provided by a phosphorus-containing compound. Preferably, the phosphorus-containing compound is selected from at least one of phosphoric acid, hypophosphorous acid, ammonium phosphate and diammonium phosphate.

[0063] In the present invention, preferably, the amounts of the Group VIII metal precursor, the Group VIB metal precursor, and the phosphorus-containing compound are such that the first hydrogenation catalyst and the second hydrogenation catalyst obtained independently satisfy the above (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value required.

[0064] According to the method of the present invention, there is no specific limitation on the impregnation method, and conventional impregnation methods in the art are applicable to the present invention. It can be co-impregnation, step-by-step impregnation, saturation impregnation, or supersaturation impregnation. Preferably, co-impregnation is adopted. Preferably, the impregnation method comprises: impregnating the aluminum oxide with an impregnation solution containing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and optionally an organic alcohol compound and / or a carboxylic acid compound.

[0065] In the present invention, there is no specific limitation on the order of adding the Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound, and optionally the organic alcohol compound and / or the carboxylic acid compound, as long as it is conducive to uniform mixing of the components. In a preferred embodiment, the organic alcohol compound and / or the carboxylic acid compound, the Group VIII metal precursor, and the Group VIB metal precursor are added to an aqueous solution of the phosphorus-containing compound to provide the impregnation solution. The order of adding the organic alcohol compound and / or the carboxylic acid compound, the phosphorus-containing compound, and the metal precursor can also be interchanged.

[0066] According to the method provided by the present invention, the prepared catalyst can have the aforementioned structure and composition according to the physical properties of the carrier and the amount of each material. The present invention has no particular limitation on this. In order to fully illustrate the technical solution of the present invention and facilitate understanding, the first hydrogenation catalyst is now taken as an example to exemplify the method provided by the present invention, but the present invention is not limited thereto. For example, the first hydrogenation catalyst can be prepared by the following preparation method: (1) Determine the amount of the VIB group metal precursor per gram of the carrier according to the atomic concentration of the VIB group metal element and the specific surface area of ​​the carrier (alumina); (2) Determine the amount of the VIII group metal precursor per gram of the carrier according to the atomic ratio of the VIII group metal element to the total amount of the VIII group metal element and the VIB group metal element; (3) Determine the amount of the VIII group metal precursor per gram of the carrier according to (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The content of P2O5 is calculated based on the value of , and then the amount of phosphorus-containing compound per gram of carrier is determined; (4) the amount of organic alcohol compound and / or carboxylic acid compound is calculated based on the molar ratio of organic alcohol compound and / or carboxylic acid compound to Group VIII metal element; (5) according to the feed amounts of Group VIB metal precursor, Group VIII metal precursor, phosphorus-containing compound and organic alcohol compound and / or carboxylic acid compound, alumina is impregnated with impregnation solution by pore saturation impregnation method, and then dried. Specifically, the phosphorus-containing compound is first dissolved in water, and then an organic alcohol compound and / or a carboxylic acid compound, a Group VIB metal precursor and a Group VIII metal precursor are added, and the mixture is stirred under heating until it is completely dissolved, and the temperature is kept constant to obtain an impregnation solution; (6) the water absorption rate of the carrier is measured, and the liquid absorption rate of the carrier is calculated according to the formula of carrier water absorption rate-0.1; (7) according to the liquid absorption rate of the carrier, the impregnation solution is adjusted to a corresponding volume (carrier liquid absorption rate×carrier mass), and the impregnation solution and the corresponding mass of the carrier are evenly mixed and allowed to stand, and then dried to prepare a catalyst.

[0067] In the present invention, the drying conditions have a wide range of selections. Preferably, the drying conditions include: a temperature of 80-200° C. and a time of 1-10 h.

[0068] The second aspect of the present invention provides a hydrorefining method, which comprises: under hydrorefining conditions, injecting a feedstock to be hydrorefined into a hydrorefining device for reaction, wherein the catalyst in the hydrorefining device is loaded according to the grading method described in the first aspect.

[0069] In the present invention, the catalyst in the hydrotreating device is the first hydrogenation catalyst and the second hydrogenation catalyst described in the first aspect of the present invention.

[0070] In the present invention, the usage of the first hydrogenation catalyst and the second hydrogenation catalyst has been described in the first aspect and will not be described again here.

[0071] According to the present invention, the hydrofining device can be selected from any conventional reactor, as long as the raw material can be contacted with the first hydrogenation catalyst and the second hydrogenation catalyst in sequence. For example, two hydrogenation reactors can be connected in series to form a first hydrogenation reaction zone and a second hydrogenation reaction zone, the first hydrogenation catalyst is loaded in the first hydrogenation reaction zone, the second hydrogenation catalyst is loaded in the second hydrogenation reaction zone, and the raw material flows through the first hydrogenation reactor and then passes into the second hydrogenation reactor for reaction. The reactor can also be divided into a first hydrogenation reaction zone and a second hydrogenation reaction zone arranged up and down, the first hydrogenation catalyst and the second hydrogenation catalyst are loaded in the two reaction zones respectively, and the raw material is injected into the reactor from top to bottom for reaction.

[0072] In a preferred case, the first hydrogenation catalyst and the second hydrogenation catalyst need to be converted from an oxidized catalyst to a sulfurized catalyst before use. In the present invention, there is no specific limitation on the sulfurization method, and conventional sulfurization methods in the art are applicable to the present invention. Preferably, for example, it can be one of dry sulfurization and wet sulfurization. There is no particular limitation on the type of the vulcanizing agent, and it can be selected according to conventional schemes in the art.

[0073] Preferably, the vulcanization conditions include: vulcanization temperature of 280-420°C, time of 10-48h, pressure of 0.1-15MPa, volume space velocity of 0.5-20h -1 , the volume ratio of hydrogen to oil is 100-2000:1, and the preferred heating rate is 5-60°C / hour.

[0074] In a preferred embodiment, the sulfur content in the raw material to be hydrotreated is 5000-30000 ppm.

[0075] In a preferred embodiment, the hydrofining conditions include: temperature of 260-410°C, pressure of 5-15 MPa, volume space velocity of 0.5-20 hours -1 , the volume ratio of hydrogen to oil is 100-2000:1.

[0076] According to the present invention, the first hydrogenation catalyst is loaded in the first hydrogenation reaction zone, and the second hydrogenation catalyst is loaded in the second hydrogenation reaction zone. Preferably, the conditions of the first hydrogenation reaction zone include: temperature of 260-380°C, pressure of 5-15 MPa, volume space velocity of 0.5-20 h -1 , the hydrogen-oil volume ratio is 100-2000:1; preferably, the conditions of the second hydrogenation reaction zone include: temperature of 350-410°C, pressure of 5-15MPa, volume space velocity of 0.5-20h -1 The volume ratio of hydrogen to oil is 100-2000:1. The above preferred implementation is beneficial to provide a better chemical reaction environment for the first hydrogenation catalyst and the second hydrogenation catalyst, and to exert the hydrodesulfurization activity and stability of the two.

[0077] The present invention will be described in detail below through examples. In the following examples, the hydrodesulfurization performance of the catalyst system is measured in a small evaluation device. The device is provided with two reactors connected in series, the first reactor is filled with the first hydrogenation catalyst of the present invention, and the second reactor is filled with the second hydrogenation catalyst of the present invention. The oxidized catalyst is directly converted into a sulfurized catalyst by a programmed temperature sulfurization method. The sulfurization conditions are: the sulfurization pressure is 6.4MPa, the sulfurized oil is kerosene containing 2% by weight of CS2, and the volume space velocity is 2h -1 , the hydrogen-to-oil ratio is 300 v / v, first keep the temperature at 230℃ / h for 6h, then increase the temperature to 360℃ for sulfidation for 8h, and the heating rate of each stage is 10℃ / h. After sulfidation, switch the reaction raw materials for hydrodesulfurization activity test, the reaction raw materials are distillate oil with a sulfur content of 10890ppm. The test conditions are: pressure of 6.4MPa, the total volume space velocity of the two reactors is 1.875h -1 , the volume ratio of hydrogen to oil is 300v / v. The properties of the product were analyzed after the reaction was stable for 2 days. In order to examine the stability of the catalyst, the mass fraction of sulfur in the reaction product was kept at 10ppm, the reaction temperature was adjusted every day, and the operation was continued for 5 days. The changes in the reaction temperature before and after 5 days were compared to measure the stability of the catalyst.

[0078] The composition of the catalyst is calculated based on the feed amount. The specific surface area, pore distribution, pore size and pore volume of the catalyst and the carrier are determined by low temperature nitrogen adsorption method (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). The sulfur mass fraction in the product is analyzed using a sulfur nitrogen analyzer (produced by Thermo Fisher, model TN / TS3000).

[0079] Example 1

[0080] The preparation process and properties of the first hydrogenation catalyst are as follows:

[0081] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0082] MoO3, basic nickel carbonate and glycerol were added to a phosphoric acid aqueous solution, heated and stirred at 85°C for 2 hours until completely dissolved and kept at a constant temperature for 3 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0083] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0084] The atomic concentration of Mo in the first hydrogenation catalyst is 7atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.29, P2O5 / MoO3 molar ratio is 0.13, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.5 nm, and the molar ratio of glycerol to Ni is 2.

[0085] After the first hydrogenation catalyst was calcined at 400°C for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst was 165m 2 / g, pore volume 0.38cm 3 / g, the average pore diameter is 9.2nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 9.2% of the total pore volume.

[0086] The preparation process and properties of the second hydrogenation catalyst are as follows:

[0087] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-20nm accounts for 66.8% of the total pore volume.

[0088] A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.

[0089] The amounts of the alumina and the components are such that the prepared catalyst satisfies:

[0090] The atomic concentration of Mo in the catalyst is 4.5atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P2O5 / MoO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.346nm, and the molar ratio of glycerol to Ni is 2.

[0091] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 192m 2 / g, pore volume 0.45cm 3 / g, the average pore diameter is 9.4nm, the pore volume with a pore diameter distribution of 8-20nm accounts for 63.0% of the total pore volume of the catalyst, and the pore diameter of the catalyst presents a single-peak pore distribution in the range of 8-20nm.

[0092] Performance testing of catalyst system:

[0093] The first hydrogenation catalyst and the second hydrogenation catalyst were compounded and loaded in a volume ratio of 1:1. The reaction temperature of the first hydrogenation catalyst was 350°C, and the reaction temperature of the second hydrogenation catalyst was 375°C. After the reaction test, the sulfur content in the product was 5.2ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 1.8°C after 5 days of reaction.

[0094] Example 2

[0095] The preparation process and properties of the first hydrogenation catalyst are as follows:

[0096] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0097] MoO3, basic nickel carbonate and glycerol were added to the phosphoric acid aqueous solution, heated and stirred at 90°C for 3 hours until completely dissolved and kept at constant temperature for 3 hours to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0098] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0099] The atomic concentration of Mo in the catalyst is 11atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.2, P2O5 / MoO3 molar ratio is 0.1, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbon fiber is 0.72 nm, and the molar ratio of glycerol to Ni is 5.

[0100] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 151m 2 / g, pore volume 0.32cm 3 / g, the average pore diameter is 8.5nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 9% of the total pore volume.

[0101] The preparation process and properties of the second hydrogenation catalyst are as follows:

[0102] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-20nm accounts for 66.8% of the total pore volume.

[0103] A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and allowed to stand for 2 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.

[0104] The amounts of the alumina and the components are such that the prepared catalyst satisfies:

[0105] The atomic concentration of Mo in the catalyst is 3atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.3, P2O5 / MoO3 molar ratio is 0.3, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbon fiber is 0.26 nm, and the molar ratio of glycerol to Ni is 5.

[0106] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 210m 2 / g, pore volume 0.5cm 3 / g, the average pore diameter is 9.5nm, the pore volume with a pore diameter distribution of 8-20nm accounts for 65.8% of the total pore volume of the catalyst, and the pore diameter of the catalyst presents a single-peak pore distribution in the range of 8-20nm.

[0107] Performance testing of catalyst system:

[0108] The first hydrogenation catalyst and the second hydrogenation catalyst were compounded and loaded in a volume ratio of 2:1. The reaction temperature of the first hydrogenation catalyst was 354°C, and the reaction temperature of the second hydrogenation catalyst was 379°C. After the reaction test, the sulfur content in the product was 4.2ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 2.1°C after 5 days of reaction.

[0109] Example 3

[0110] The preparation process and properties of the first hydrogenation catalyst are as follows:

[0111] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0112] MoO3, basic nickel carbonate and glycerol were added to a phosphoric acid aqueous solution, heated and stirred at 90°C for 3 hours until completely dissolved and kept at a constant temperature for 3 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 2 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0113] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0114] The atomic concentration of Mo in the catalyst is 8atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.28, P2O5 / MoO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbon fiber is 0.623 nm, and the molar ratio of glycerol to Ni is 3.

[0115] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 164m 2 / g, pore volume 0.35cm 3 / g, the average pore diameter is 8.5nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 8% of the total pore volume.

[0116] The preparation process and properties of the second hydrogenation catalyst are as follows:

[0117] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-20nm accounts for 66.8% of the total pore volume.

[0118] A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 95°C for 2 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 4 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.

[0119] The amounts of the alumina and the components are such that the prepared catalyst satisfies:

[0120] The atomic concentration of Mo in the catalyst is 3.5atom / nm 2, Ni / (Ni+Mo) atomic ratio is 0.28, P2O5 / MoO3 molar ratio is 0.25, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbon fiber is 0.29 nm, and the molar ratio of glycerol to Ni is 3.

[0121] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 204m 2 / g, pore volume 0.48cm 3 / g, the average pore diameter is 9.4nm, the pore volume with a pore diameter distribution of 8-20nm accounts for 66.2% of the total pore volume of the catalyst, and the pore diameter of the catalyst presents a single-peak pore distribution in the range of 8-20nm.

[0122] Performance testing of catalyst system:

[0123] The first hydrogenation catalyst and the second hydrogenation catalyst were compounded and loaded in a volume ratio of 1:2. The reaction temperature of the first hydrogenation catalyst was 345°C, and the reaction temperature of the second hydrogenation catalyst was 370°C. After the reaction test, the sulfur content in the product was 7.8ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 2.3°C after 5 days of reaction.

[0124] Example 4

[0125] The preparation process and properties of the first hydrogenation catalyst are as follows:

[0126] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0127] Ammonium metatungstate, basic nickel carbonate and citric acid were added to the phosphoric acid aqueous solution respectively, heated and stirred at 90°C for 2 hours until completely dissolved and kept at constant temperature for 3 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 2 hours, and dried at 130°C for 3 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.

[0128] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0129] The atomic concentration of W in the catalyst is 5atom / nm 2, Ni / (Ni+W) atomic ratio is 0.3, P2O5 / WO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.407 nm, and the molar ratio of citric acid to Ni is 2.

[0130] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 162m 2 / g, pore volume 0.39cm 3 / g, the average pore diameter is 9.6nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 10.5% of the total pore volume.

[0131] The preparation process and properties of the second hydrogenation catalyst are as follows:

[0132] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-20nm accounts for 66.8% of the total pore volume.

[0133] A certain amount of ammonium metatungstate, basic nickel carbonate and citric acid were added to the aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 2 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.

[0134] The amounts of the alumina and the components are such that the prepared catalyst satisfies:

[0135] The atomic concentration of W in the catalyst is 4atom / nm 2 , Ni / (Ni+W) atomic ratio is 0.3, P2O5 / WO3 molar ratio is 0.35, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.38 nm, and the molar ratio of citric acid to Ni is 2.

[0136] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 170m 2 / g, pore volume 0.4cm3 / g, the average pore diameter is 9.4nm, the pore volume with a pore diameter distribution of 8-20nm accounts for 65.8% of the total pore volume of the catalyst, and the pore diameter of the catalyst presents a single-peak pore distribution in the range of 8-20nm.

[0137] Performance testing of catalyst system:

[0138] The first hydrogenation catalyst and the second hydrogenation catalyst were compounded and loaded in a volume ratio of 1:3. The reaction temperature of the first hydrogenation catalyst was 343°C, and the reaction temperature of the second hydrogenation catalyst was 368°C. After the reaction test, the sulfur content in the product was 6.5ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 2.0°C after 5 days of reaction.

[0139] Example 5

[0140] The preparation process and properties of the first hydrogenation catalyst are as follows:

[0141] The γ-alumina carrier was selected, with a water absorption rate of 1.04 mL / g and a specific surface area of ​​270 m 2 / g, the average pore size is 11.7nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0142] MoO3, basic nickel carbonate and citric acid were added to a phosphoric acid aqueous solution, heated and stirred at 85°C for 3 hours until completely dissolved and kept at a constant temperature for 2 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0143] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0144] The atomic concentration of Mo in the catalyst is 9atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P2O5 / MoO3 molar ratio is 0.12, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.62 nm, and the molar ratio of citric acid to Ni is 2.

[0145] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 154m 2 / g, pore volume 0.36cm 3 / g, the average pore diameter is 9.4nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 9.8% of the total pore volume.

[0146] The preparation process and properties of the second hydrogenation catalyst are as follows:

[0147] The γ-alumina carrier was selected, with a water absorption rate of 1.04 mL / g and a specific surface area of ​​270 m 2 / g, the average pore size is 11.7nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-2nm accounts for 73.5% of the total pore volume.

[0148] A certain amount of MoO3, basic nickel carbonate and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 4 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.

[0149] The amounts of the alumina and the components are such that the prepared catalyst satisfies:

[0150] The atomic concentration of Mo in the catalyst is 4.2atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P2O5 / MoO3 molar ratio is 0.32, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.37 nm, and the molar ratio of citric acid to Ni is 2.

[0151] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 189m 2 / g, pore volume 0.48cm 3 / g, the average pore size is 10.2nm, the pore volume with a pore size distribution of 8-20nm accounts for 69.5% of the total pore volume of the catalyst, and the pore size of the catalyst presents a single-peak pore distribution in the range of 8-20nm.

[0152] Performance testing of catalyst system:

[0153] The first hydrogenation catalyst and the second hydrogenation catalyst were compounded and loaded in a volume ratio of 3:1. The reaction temperature of the first hydrogenation catalyst was 356°C, and the reaction temperature of the second hydrogenation catalyst was 381°C. After the reaction test, the sulfur content in the product was 4.7ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 2.1°C after 5 days of reaction.

[0154] Example 6

[0155] The preparation process and properties of the first hydrogenation catalyst are as follows:

[0156] The γ-alumina carrier was selected, with a water absorption rate of 1.04 mL / g and a specific surface area of ​​270 m 2 / g, the average pore size is 11.7nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0157] MoO3, basic nickel carbonate and citric acid were added to a phosphoric acid aqueous solution, heated and stirred at 95°C for 3 hours until completely dissolved and kept at a constant temperature for 2 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0158] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0159] The atomic concentration of Mo in the catalyst is 10atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.28, P2O5 / MoO3 molar ratio is 0.27, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.85 nm, and the molar ratio of citric acid to Ni is 2.

[0160] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 135m 2 / g, pore volume 0.27cm 3 / g, the average pore diameter is 8.0nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 12.5% ​​of the total pore volume.

[0161] The preparation process and properties of the second hydrogenation catalyst are as follows:

[0162] The γ-alumina carrier was selected, with a water absorption rate of 1.04 mL / g and a specific surface area of ​​270 m 2 / g, the average pore size is 11.7nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm, accounting for 73.5%.

[0163] A certain amount of MoO3, basic nickel carbonate and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.

[0164] The amounts of the alumina and the components are such that the prepared catalyst satisfies:

[0165] The atomic concentration of Mo in the catalyst is 4.5atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.2, P2O5 / MoO3 molar ratio is 0.25, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.36 nm, and the molar ratio of citric acid to Ni is 2.

[0166] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 190m 2 / g, pore volume 0.47cm 3 / g, the average pore diameter is 9.9nm, the pore volume with a pore diameter distribution of 8-20nm accounts for 72.6% of the total pore volume of the catalyst, and the pore diameter of the catalyst presents a single-peak pore distribution in the range of 8-20nm.

[0167] Performance testing of catalyst system:

[0168] The first hydrogenation catalyst and the second hydrogenation catalyst were compounded and loaded in a volume ratio of 1:4. The reaction temperature of the first hydrogenation catalyst was 342°C, and the reaction temperature of the second hydrogenation catalyst was 367°C. After the reaction test, the sulfur content in the product was 8.6ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 1.9°C after 5 days of reaction.

[0169] Comparative Example 1

[0170] The preparation process and properties of the first hydrogenation catalyst are as follows:

[0171] The same carrier as the first hydrogenation catalyst in Example 1 was selected to prepare a catalyst. MoO3, basic nickel carbonate, and glycerol were added to a phosphoric acid aqueous solution, heated and stirred at 85°C for 2 hours until completely dissolved and kept at a constant temperature for 3 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 2 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0172] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0173] The atomic concentration of Mo in the catalyst is 4atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.22, P2O5 / MoO3 molar ratio is 0.3, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.34 nm, and the molar ratio of glycerol to Ni is 2.

[0174] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 205m 2 / g, pore volume 0.48cm 3 / g, the average pore size is 9.5nm, the pore size distribution of the catalyst is a single-peak pore, and the position of the single-peak pore is 8.9nm.

[0175] The preparation process and properties of the second bed catalyst are as follows:

[0176] The same carrier as the second hydrogenation catalyst in Example 1 was selected to prepare a catalyst. A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.

[0177] The amounts of the alumina and the components are such that the prepared catalyst satisfies:

[0178] The atomic concentration of Mo in the catalyst is 2atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.22, P2O5 / MoO3 molar ratio is 0.3, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.17 nm, and the molar ratio of glycerol to Ni is 2.

[0179] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 230m 2 / g, pore volume 0.58cm 3 / g, the average pore diameter is 10.1nm, the pore volume with a pore diameter distribution of 8-20nm accounts for 66.2% of the total pore volume of the catalyst, and the pore diameter of the catalyst presents a single-peak pore distribution in the range of 8-20nm.

[0180] Performance testing of catalyst system:

[0181] The first hydrogenation catalyst and the second hydrogenation catalyst were compounded and loaded in a volume ratio of 1:1. The reaction temperature of the first hydrogenation catalyst was 350°C, and the reaction temperature of the second hydrogenation catalyst was 375°C. After the reaction test, the sulfur content in the product was 26.5ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 2.6°C after 5 days of reaction.

[0182] Comparative Example 2

[0183] The first hydrogenation catalyst and the second hydrogenation catalyst in Implementation 1 were selected, and the first hydrogenation catalyst and the second hydrogenation catalyst were compounded and loaded according to a volume ratio of 5:1. The reaction temperature of the first hydrogenation catalyst was 358°C, and the reaction temperature of the second hydrogenation catalyst was 383°C. After the reaction test, the sulfur content in the product was 15.3ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 2.9°C after 5 days of reaction.

[0184] It can be seen from the examples and comparative examples that the present invention has good inventive effects, the prepared catalyst system has high activity and stability, and has good industrial application prospects.

[0185] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for grading a hydrotreating catalyst, the method comprising: A first hydrogenation catalyst and a second hydrogenation catalyst are sequentially loaded along the direction of the logistics; The packing volume ratio of the first hydrogenation catalyst to the second hydrogenation catalyst is 1:4-4:1; The first hydrogenation catalyst comprises at least one Group VIII metal element, at least one Group VIB metal element and alumina, and the pore size of the first hydrogenation catalyst is in the range of 2-6 nm and 8-20 nm, presenting a bimodal pore distribution; The volume of pores with a pore size distribution of 2-6 nm in the first hydrogenation catalyst accounts for 8-15% of the total pore volume of the catalyst; The specific surface area of ​​the first hydrogenation catalyst is 130-170m 2 / g; The pore volume of the first hydrogenation catalyst is 0.25-0.4 cm 3 / g; The average pore size of the first hydrogenation catalyst is 8-10 nm; The second hydrogenation catalyst comprises alumina and a Group VIII metal element and a Group VIB metal element supported on the alumina, and the pore size of the second hydrogenation catalyst is in the range of 8-20 nm and presents a unimodal pore distribution; The volume of pores with a pore size distribution of 8-20 nm in the second hydrogenation catalyst accounts for 50-80% of the total pore volume of the catalyst; The specific surface area of ​​the second hydrogenation catalyst is 185-210m 2 / g; The pore volume of the second hydrogenation catalyst is 0.4-0.6 cm 3 / g; The average pore diameter of the second hydrogenation catalyst is 6-18 nm.

2. The method according to claim 1, wherein: The packing volume ratio of the first hydrogenation catalyst to the second hydrogenation catalyst is 1:3-3:

1.

3. The method according to claim 1 or 2, wherein: The equivalent diameters of the first hydrogenation catalyst and the second hydrogenation catalyst are each independently 0.5-1.8 mm.

4. The method according to claim 3, wherein: The equivalent diameters of the first hydrogenation catalyst and the second hydrogenation catalyst are each independently 0.8-1.6 mm.

5. The method according to claim 1 or 2, wherein: The shapes of the first hydrogenation catalyst and the second hydrogenation catalyst are independently butterfly-shaped, cylindrical, four-leaf clover-shaped, honeycomb-shaped or other irregular shapes.

6. The method according to claim 1 or 2, wherein: The volume of pores with pore diameter distribution in the range of 2-6 nm in the first hydrogenation catalyst accounts for 9-12% of the total pore volume of the catalyst.

7. The method according to claim 1 or 2, wherein: The first hydrogenation catalyst composition is (Xi ai )•(Yi bi )•(Zi ci )•Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of the carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of the carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of the carrier P2O5, Sup refers to the carrier, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.4-0.9nm, ρ Xi , Yi , Zi are the densities of VIB group metal oxides, VIII group metal oxides and P2O5, SA sup is the specific surface area of ​​the carrier.

8. The method according to claim 7, wherein: The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value is 0.5-0.8nm.

9. The method according to claim 7, wherein: The molar ratio of Zi / Xi in the first hydrogenation catalyst is 0.05-0.

3.

10. The method according to claim 9, wherein: The molar ratio of Zi / Xi in the first hydrogenation catalyst is 0.08-0.

2.

11. The method according to claim 1 or 2, wherein: The volume of pores with pore diameter distribution in the range of 8-20 nm in the second hydrogenation catalyst accounts for 60-75% of the total pore volume of the catalyst.

12. The method according to claim 1 or 2, wherein: The second hydrogenation catalyst composition is (Xi ai )•(Yi bi )•(Zi ci )•Sup represents, where Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of carrier P2O5, Sup refers to the carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.18-0.39nm, ρ Xi , Yi , Zi are the densities of VIB group metal oxides, VIII group metal oxides and P2O5, SA sup is the specific surface area of ​​the carrier.

13. The method according to claim 12, wherein: The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value is 0.25-0.38nm.

14. The method according to claim 12, wherein: The molar ratio of Zi / Xi in the second hydrogenation catalyst is 0.1-0.35:

1.

15. The method according to claim 14, wherein: The molar ratio of Zi / Xi in the second hydrogenation catalyst is 0.2-0.35:

1.

16. The method according to claim 1 or 2, wherein:The first hydrogenation catalyst and the second hydrogenation catalyst use the same alumina, the water absorption rate of the alumina used is greater than 0.9 mL / g, and the specific surface area is greater than 260 m 2 / g, the average pore size is greater than 8nm, and the pore distribution morphology is a unimodal pore distribution.

17. The method according to claim 16, wherein: In the alumina, the volume of pores with pore diameter distribution in the range of 2-6 nm accounts for no more than 10% of the total pore volume of the alumina.

18. The method according to claim 17, wherein: In the alumina, the volume of pores with pore diameter distribution in the range of 2-6 nm accounts for no more than 8% of the total pore volume of the alumina.

19. The method according to claim 1 or 2, wherein: In the alumina, the volume of pores with pore diameter distribution in the range of 2-4 nm accounts for no more than 4% of the total pore volume of the alumina.

20. The method according to claim 19, wherein: In the alumina, the volume of pores with pore diameter distribution in the range of 2-4 nm accounts for no more than 2% of the total pore volume of the alumina.

21. The method according to claim 1 or 2, wherein: The atomic concentration of the VIB group metal element on the carrier surface in the first hydrogenation catalyst is 5-13 atom / nm 2 ; and / or, the atomic concentration of the metal element of Group VIB in the second hydrogenation catalyst on the surface of the carrier is 2-6atom / nm 2 .

22. The method according to claim 21, wherein: The atomic concentration of the VIB group metal element on the carrier surface in the first hydrogenation catalyst is 5-11 atom / nm 2 .

23. The method according to claim 21, wherein: The atomic concentration of the VIB group metal element on the surface of the carrier in the second hydrogenation catalyst is 3-4.5 atom / nm 2 .

24. The method according to claim 1 or 2, wherein: The atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the first hydrogenation catalyst is 0.05-0.35; and / or the atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the second hydrogenation catalyst is 0.2-0.

4.

25. The method according to claim 24, wherein: The atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the first hydrogenation catalyst is 0.1-0.

3.

26. The method according to claim 24, wherein: The atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the second hydrogenation catalyst is 0.2-0.

35.

27. The method according to claim 1 or 2, wherein: The first hydrogenation catalyst and the second hydrogenation catalyst each independently include an organic alcohol compound and / or a carboxylic acid compound.

28. The method according to claim 27, wherein: In the first hydrogenation catalyst and the second hydrogenation catalyst, the molar ratio of the organic alcohol compound and / or the carboxylic acid compound to the Group VIII metal element is independently 1-6.

29. The method according to claim 28, wherein: In the first hydrogenation catalyst and the second hydrogenation catalyst, the molar ratio of the organic alcohol compound and / or the carboxylic acid compound to the Group VIII metal element is independently 2-5.

30. The method according to claim 1 or 2, wherein: The preparation methods of the first hydrogenation catalyst and the second hydrogenation catalyst each independently comprise: introducing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound and optionally an organic alcohol compound and / or a carboxylic acid compound into alumina by an impregnation method, and then drying.

31. A hydrofining method, the method comprising: Under hydrorefining conditions, the raw material to be hydrorefined is injected into a hydrorefining device for reaction, wherein the catalyst in the hydrorefining device is loaded according to the grading method described in any one of claims 1 to 30.

32. The purification method according to claim 31, wherein The sulfur content of the raw material to be hydrorefined is 5000-30000 ppm.

33. The purification method according to claim 31 or 32, wherein: The hydrofining conditions include: temperature of 260-410°C, pressure of 5-15 MPa, volume space velocity of 0.5-20 hours -1 , the volume ratio of hydrogen to oil is 100-2000:1.