Catalyst and its preparation method and application
By using silicon carbide whiskers as a support catalyst, the problem of poor heat transfer in the process of oxidizing benzene partly is solved, and the reaction heat is removed in a timely manner, which improves the selectivity and yield of the manganese anhydride and significantly improves the craft benefits.
Patent Information
- Application Number
- CN202111284629.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-01
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-11-01
AI Technical Summary
In the prior art, the catalyst heat transfer is poor in the process of oxidizing benzene partially, resulting in overheating of the catalyst bed and producing a large amount of carbon monoxide and carbon dioxide, affecting the process benefits.
Silicon carbide whiskers are used as support to spray and activate the active components to prepare a catalyst with good thermal conductivity to ensure that the reaction heat is removed in time and improve the catalyst stability and selectivity of the manic anhydride.
It effectively reduces the by-product of benzene, improves the selectivity and yield of maleic anhydride, maintains the high stability of the catalyst, and improves the economic benefits of the process.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to a catalyst and a preparation method and application thereof. Background Art
[0002] Maleic anhydride (maleic anhydride) is a very important organic chemical raw material and the second largest organic anhydride after phthalic anhydride. It has a wide range of uses and can be used to produce 1,4-butanediol, tetrahydrofuran, γ-butyrolactone, malic acid, unsaturated polyester resin, etc. It can also be used as a raw material for medicine and pesticides. Unsaturated polyester resin (UPR) is the largest downstream consumer product of maleic anhydride, followed by 1,4-butanediol. The consumption of the two can account for more than 60% of the total consumption of maleic anhydride.
[0003] The production process of maleic anhydride can be divided into benzene process and butane process according to the different raw materials. In recent years, the production capacity of domestic n-butane oxidation process has been continuously expanded, and the development momentum is relatively fast. However, the n-butane process of maleic anhydride is more complicated than the benzene process and is relatively difficult to operate. Therefore, the process using benzene as raw material still accounts for 50% of the total maleic anhydride production capacity.
[0004] In areas where coal resources are relatively abundant and oil resources are relatively scarce, coal chemical production capacity is high and a large amount of coking benzene will be produced. Due to the raw material advantage, the process of using coking benzene as raw material to produce maleic anhydride in this area has occupied the mainstream process. At present, when the price difference between the benzene raw material cost and the maleic anhydride product is small, there is a very large competition among enterprises in production. In order to improve the economic benefits of the device, it is necessary to reduce production costs as much as possible, reduce benzene consumption, reduce benzene by-products, and improve the selectivity of maleic anhydride, which can significantly improve the economic benefits of the benzene-based maleic anhydride device.
[0005] The partial oxidation of benzene to produce maleic anhydride is a violent reaction process that generates a large amount of heat. If the heat cannot be removed in time during the production process, it will cause local overheating of the catalyst bed, and benzene and maleic anhydride will burn violently under high temperature conditions, producing a large amount of carbon monoxide and carbon dioxide as by-products. Therefore, it is very important to remove the heat generated by the reaction process in time for the partial oxidation of benzene. Summary of the invention
[0006] The purpose of the present invention is to overcome the problem of catalyst heat transfer in the prior art and to provide a catalyst and a preparation method and application thereof, which can remove the heat generated by the reaction in a timely manner, thereby improving the performance of the catalyst and maintaining a high stability of the catalyst.
[0007] The inventors found during the research that the partial oxidation of benzene to produce maleic anhydride is a violent reaction process that generates a large amount of heat. If the heat cannot be removed in time during the production process, the catalyst bed will be locally overheated, and benzene and maleic anhydride will burn violently under high temperature conditions, producing a large amount of carbon monoxide and carbon dioxide as by-products. Therefore, it is very important to remove the heat generated in the reaction process in time for the partial oxidation of benzene to produce maleic anhydride.
[0008] Silicon carbide is a kind of inert carrier, because of its small specific surface area, good thermal conductivity, high mechanical strength advantages, therefore used for the carrier of benzene oxidation catalyst for maleic anhydride.And the inventor disclosed a catalyst and its preparation method and application (CN109201095A) utilizing benzene oxidation for maleic anhydride in the previous application, the catalyst active component is sprayed on the silicon carbide carrier, and the catalyst is prepared through activation.Although the carrier in this catalyst is silicon carbide, the specific kind of silicon carbide is not disclosed, the inventor continues to study on this basis, surprisingly finds that the carrier prepared by raw material is silicon carbide whisker, utilizes the good thermal conductivity of silicon carbide whisker, lower specific surface area and higher intensity, can effectively remove the heat generated by reaction in time, thereby improves the performance of catalyst, keeps the higher stability of catalyst.
[0009] In order to achieve the above object, the present invention provides a catalyst on one hand, which comprises a carrier and an active component supported on the carrier, wherein the carrier comprises silicon carbide whiskers.
[0010] The second aspect of the present invention provides a method for preparing a catalyst, which comprises loading an active component precursor on a carrier and then activating the carrier; wherein the carrier contains silicon carbide whiskers.
[0011] The third aspect of the present invention provides a catalyst prepared by the above method.
[0012] A fourth aspect of the present invention provides a use of the above catalyst in the preparation of maleic anhydride.
[0013] Through the above technical solution, the present invention achieves the following beneficial effects:
[0014] (1) The carrier prepared by the present invention has easy-to-obtain raw materials, a simple preparation process, and easy-to-control conditions.
[0015] (2) Nano-scale silicon carbide whiskers are used as carriers to improve the heat transfer performance of the carrier, transfer the reaction heat in time, reduce the heat generated by the benzene oxidation reaction, reduce the peroxidation of benzene, and improve the selectivity of maleic anhydride.
[0016] (3) Nano-scale silicon carbide whiskers are used as the main raw material of the carrier, and porcelain clay, methyl cellulose, polypropylene and silica sol are used as auxiliary raw materials to prepare the carrier. No significant changes are made to the existing process. The process technology is mature and the cost is low.
[0017] (4) The selectivity and yield of maleic anhydride can be further improved by using the carrier prepared from the silicon carbide whisker of the present invention as a raw material and compounding the catalyst of the first active component and the second active component. DETAILED DESCRIPTION
[0018] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0019] A first aspect of the present invention provides a catalyst comprising a carrier and an active component supported on the carrier, wherein the carrier contains silicon carbide whiskers.
[0020] According to the present invention, preferably, the length of the silicon carbide whisker is 2-50 μm, the particle size is 50-500 nm, the aspect ratio is 20-200, and the crystal form of the silicon carbide whisker is α-type and / or β-type.
[0021] In the present invention, "grain size of silicon carbide whiskers" refers to "diameter of silicon carbide whiskers", and "aspect ratio" refers to the ratio of "length" to "grain size" of silicon carbide whiskers.
[0022] According to the present invention, preferably, the carrier further contains alumina and / or silica.
[0023] According to the present invention, preferably, the active component is selected from at least one of Group VB metal compounds, Group VIB metal compounds, Group IA metal compounds, Group IIIA metal compounds, Group VA non-metal compounds and Group VIII metal compounds.
[0024] According to the present invention, preferably, with respect to every 100 g of the catalyst, the content of the active component is 10-30 g, and the content of the carrier is 70-90 g.
[0025] According to the present invention, preferably, the content of the silicon carbide whisker is 65-95 g, preferably 80-94 g, per 100 g of the carrier.
[0026] According to the present invention, preferably, the active component includes a first active component and a second active component, the first active component includes at least one of vanadium oxide, molybdenum oxide, sodium oxide, phosphorus oxide and nickel oxide, and the second active component includes at least one of indium oxide, antimony oxide and bismuth oxide.
[0027] According to the present invention, preferably, the active components include the contents of each substance in the first active component and the second active component: vanadium oxide calculated as V2O5, molybdenum oxide calculated as MoO3, sodium oxide calculated as Na2O, phosphorus oxide calculated as P2O5, nickel oxide calculated as NiO and the molar ratio of the second active component calculated as metal oxide is 1: (0.2-0.9): (0.001-0.2): (0.005-0.25): (0.0001-0.05): (0.0001-0.05).
[0028] The second aspect of the present invention provides a method for preparing a catalyst, which comprises loading an active component precursor on a carrier and then activating the carrier; wherein the carrier contains silicon carbide whiskers.
[0029] According to the present invention, preferably, the length of the silicon carbide whisker is 2-50 μm, the particle size is 50-500 nm, the aspect ratio is 20-200, and the crystal form of the silicon carbide whisker is α and / or β type.
[0030] According to the present invention, preferably, the carrier further contains alumina and / or silica.
[0031] According to the present invention, preferably, the content of the silicon carbide whisker is 65-95 g, preferably 80-94 g, per 100 g of the carrier.
[0032] According to the present invention, preferably, the carrier is obtained by mixing silicon carbide whiskers, china clay, methyl cellulose, polypropylene and silica sol, and then performing a first drying and calcining to obtain the carrier.
[0033] According to the present invention, preferably, the content of silicon dioxide in the silica sol is 8-12% by weight.
[0034] According to the present invention, preferably, the weight ratio of the silicon carbide whisker, china clay, methyl cellulose, polypropylene and silica sol is 15-45:1-2:0.5-1.5:0.5-1.5:1.
[0035] According to the present invention, preferably, the first drying is carried out at a temperature of 100-150° C. and for a time of 6-10 h.
[0036] According to the present invention, preferably, the calcination temperature is 800-1200° C. and the calcination time is 3-8 hours.
[0037] According to the present invention, preferably, the active component precursor is selected from at least one of Group VB metal compounds, Group VIB metal compounds, Group IA metal compounds, Group IIIA metal compounds, Group VA non-metal compounds and Group VIII metal compounds.
[0038] According to the present invention, preferably, the active component precursor includes a first active component precursor and a second active component precursor, the first active component precursor includes at least one of a vanadium compound, a molybdenum compound, a sodium compound, a phosphorus compound and a nickel compound, and the second active component precursor includes at least one of an indium compound, an antimony compound and a bismuth compound.
[0039] According to the present invention, preferably, the molar ratio of the amounts of the first active component precursor and the second active component precursor: the vanadium compound calculated as V2O5, the molybdenum compound calculated as MoO3, the sodium compound calculated as Na2O, the phosphorus compound calculated as P2O5, the nickel compound calculated as NiO and the second active component precursor calculated as metal oxide is 1: (0.2-0.9): (0.001-0.2): (0.00 5-0.25):(0.0001-0.05):(0.0001-0.05); more preferably 1:(0.4-0.6):(0.1-0.15):(0.02-0.25):(0.01-0.02):(0.003-0.02); wherein, the indium compound in the second active component precursor is calculated as In2O3, the antimony compound is calculated as Sb2O3, and the bismuth compound is calculated as Bi2O3.
[0040] According to the present invention, preferably, the vanadium compound is at least one of ammonium metavanadate, vanadium pentoxide and sodium vanadate, preferably ammonium metavanadate.
[0041] According to the present invention, preferably, the molybdenum compound is at least one of ammonium molybdate, molybdenum trioxide and calcium molybdate, preferably ammonium molybdate.
[0042] According to the present invention, preferably, the sodium compound is sodium dihydrogen phosphate and / or trisodium phosphate, preferably trisodium phosphate.
[0043] According to the present invention, preferably, the phosphorus compound is at least one of diammonium phosphate, phosphoric acid and phosphorus pentoxide.
[0044] According to the present invention, preferably, the nickel compound is at least one of nickel nitrate, nickel sulfate, nickel chloride and nickel oxide, more preferably nickel nitrate.
[0045] According to the present invention, preferably, the loading method is: coating the carrier with a solution containing the active component precursor.
[0046] According to the present invention, preferably, a solution containing an active component precursor is coated on a carrier to obtain a catalyst precursor, and the catalyst precursor is activated to obtain a catalyst. Based on the total weight of the catalyst precursor, the content of the active component precursor is 16-18% by weight.
[0047] According to the present invention, preferably, the method for preparing the solution containing the active component precursor is: sequentially adding the first active component precursor and the second active component precursor to the reducing agent solution.
[0048] According to the present invention, preferably, the reducing agent solution is an aqueous oxalic acid solution.
[0049] According to the present invention, preferably, the mass percentage of the reducing agent solution is 10-20wt%.
[0050] According to the present invention, preferably, the coating conditions include: a temperature of 250-300°C.
[0051] According to the present invention, the equipment used for the coating is not particularly limited, as long as the active component can be loaded on the carrier. Preferably, the coating is carried out in a stainless steel drum that can rotate and be heated, and a thermocouple sleeve is provided in the stainless steel drum for heating the carrier. The temperature of the thermocouple sleeve is controllable and has a temperature display, and the change of the carrier temperature can be detected in real time during the coating process. The active component is sprayed onto the carrier through a nozzle to complete the coating, and then a second drying is performed to obtain the catalyst. Wherein, the conditions of the second drying include: a temperature of 100-150°C and a time of 2-8h.
[0052] According to the present invention, preferably, during the coating process, the rotation speed of the stainless steel drum is 15-40 rpm / min, when the carrier is heated to 250-270°C, the spraying temperature is 250-300°C, and the carrier temperature is maintained at 260-270°C.
[0053] According to the present invention, preferably, the activation conditions include: temperature of 420-470° C. and time of 5-10 h.
[0054] According to the present invention, preferably, the activation conditions further include: a programmed temperature increase process and a programmed temperature decrease process.
[0055] According to the present invention, preferably, the programmed temperature rising process comprises heating from room temperature to 140-160°C at a heating rate of 60-120°C / h, maintaining for 5-30min, then heating to 240-260°C at a heating rate of 50-110°C / h, maintaining for 5-30min, then heating to 340-360°C at a heating rate of 40-100°C / h, maintaining for 10-60min, and finally heating to 420-470°C at a heating rate of 30-90°C / h.
[0056] According to the present invention, preferably, the programmed cooling process includes cooling to room temperature at a rate of 40-90°C / h.
[0057] According to the present invention, preferably, the activation is performed under an inert atmosphere, and further preferably, the inert atmosphere is selected from nitrogen and / or helium atmosphere.
[0058] According to the present invention, preferably, the activation is carried out in a sealed container. The sealed container is a cylindrical or cubic activation furnace body, the upper part of the furnace body is sealed by a flange to isolate the internal space from the outside, the outer wall of the furnace body is wrapped with electric furnace wires, and the outside of the electric furnace wires is provided with insulation cloth or insulation tiles, and the heating temperature of the furnace body is controlled by an automated digital temperature controller; the furnace body is provided with vents at the top and bottom, the lower vent is used as a gas inlet, and the upper vent is used as a gas outlet, and the gas flow rate is controlled by a gas mass flow meter.
[0059] The third aspect of the present invention provides a catalyst prepared by the above method.
[0060] A fourth aspect of the present invention provides a use of the above catalyst in the preparation of maleic anhydride.
[0061] According to the present invention, preferably, the catalyst is used in the reaction conditions of benzene oxidation to maleic anhydride including: molten salt temperature of 340-360°C, benzene concentration of 40-55g / Nm 3 , the volume space velocity of oxygen is 300-600h -1 , preferably 400-500h -1 .
[0062] In the present invention, the concentration of benzene refers to the mass number of benzene contained in unit volume of air, measured in grams. The higher the value, the higher the benzene content.
[0063] The oxygen in the present invention can be provided in the form of oxygen-containing gas or in the form of pure oxygen. Preferably, the oxygen is provided in the form of air. More preferably, the volume space velocity of the air is 1500-3000h / min. -1 , preferably 2000-2500h -1 .
[0064] According to the present invention, the pressure of the catalyst in the reaction of benzene oxidation to maleic anhydride is not particularly limited, and the reaction can be carried out under negative pressure, normal pressure and pressurized conditions. Preferably, the catalyst is usually used in the reaction of benzene oxidation to maleic anhydride under normal pressure.
[0065] According to the present invention, the reactor for the benzene oxidation to maleic anhydride reaction is not particularly limited and can be a reactor commonly used in the art, such as a fixed bed reactor. Preferably, the fixed bed reactor is provided with a bubbling molten salt circulation reaction tube; the bottom and the top of the reaction tube are filled with an inert carrier support, and the middle is filled with a catalyst, wherein the inert carrier is a silicon carbide carrier.
[0066] In the present invention, during the reaction process of benzene oxidation to maleic anhydride, the temperature of the catalyst at various locations in the bed is inconsistent, wherein the highest value of the temperature region is called the hot spot temperature of the catalyst, and the corresponding bed height is the hot spot position of the catalyst. In the present invention, a thermocouple is used to measure the bed temperature by pulling. Preferably, during the reaction process of benzene oxidation to maleic anhydride, the hot spot temperature is 450-460°C.
[0067] The present invention will be described in detail below by way of examples. In the following examples,
[0068] The room temperature is about "25°C";
[0069] The china clay was a commercial product of Aladdin Company with the brand number K100133;
[0070] Methylcellulose is a commercial product of Aladdin Company with the brand number M112868;
[0071] Polypropylene is a commercial product of Aladdin Company with the brand number P110853;
[0072] Silica sol (the content of silicon dioxide in the silica sol is 10%) is a commercial product of Inotech with the brand number I03052;
[0073] The contents of benzene and maleic anhydride in the reaction product were analyzed by gas chromatography.
[0074] Benzene conversion rate (%) = (the amount of benzene at the reactor inlet per unit time - the amount of benzene at the reactor outlet per unit time) / the amount of benzene at the reactor inlet per unit time × 100%;
[0075] Maleic anhydride selectivity (%) = the amount of benzene converted into maleic anhydride per unit time / (the amount of benzene at the reactor inlet per unit time - the amount of benzene at the reactor outlet per unit time) × 100%;
[0076] Maleic anhydride yield (%) = the amount of benzene converted into maleic anhydride per unit time / the amount of benzene at the reactor inlet per unit time × 100%.
[0077] Preparation Example 1
[0078] Take 400g of silicon carbide whiskers with a particle size of 50nm and a length of 2μm, add 25g of kaolin, 25g of methyl cellulose, 25g of polypropylene and 25g of silica sol, and then add 90mL of water, mix, stir and knead into a ring-shaped carrier, dry at 120°C for 8h, and calcine at 1000°C for 5h to obtain a carrier.
[0079] Preparation Example 2
[0080] Take 375g of silicon carbide whiskers with a particle size of 500nm and a length of 50μm, add 50g of kaolin, 25g of methyl cellulose, 25g of polypropylene and 25g of silica sol, and then add 90mL of water, mix, stir and knead into a ring-shaped carrier, dry at 130°C for 9h, and calcine at 1100°C for 6h to obtain a carrier.
[0081] Preparation Example 3
[0082] Take 450g of silicon carbide whiskers with a particle size of 300nm and a length of 25μm, add 20g of kaolin, 10g of methyl cellulose, 10g of polypropylene and 10g of silica sol, and then add 90mL of water, mix, stir and knead into a ring-shaped carrier, dry at 140°C for 7h, and calcine at 1000°C for 7h to obtain a carrier.
[0083] Preparation Example 4
[0084] Take 400g of silicon carbide whiskers with a particle size of 50nm and a length of 2μm, add 25g of china clay, 25g of methyl cellulose, 25g of polypropylene and 25g of silica sol, and then add 90mL of water, mix, stir and knead into a ring-shaped carrier, dry at 100℃ for 10h, and calcine at 1200℃ for 3h to obtain a carrier.
[0085] Preparation Example 5
[0086] Take 400g of silicon carbide whiskers with a particle size of 100nm and a length of 20μm, add 25g of kaolin, 25g of methyl cellulose, 25g of polypropylene and 25g of silica sol, and then add 90mL of water, mix, stir and knead into a ring-shaped carrier, dry at 150°C for 6h, and calcine at 800°C for 8h to obtain a carrier.
[0087] Preparation Example 6
[0088] Take 400g of silicon carbide whiskers with a particle size of 75nm and a length of 2μm, add 25g of kaolin, 20g of methyl cellulose, 20g of polypropylene and 25g of silica sol, and then add 90mL of water, mix, stir and knead into a ring-shaped carrier, dry at 120°C for 8h, and calcine at 1000°C for 5h to obtain a carrier.
[0089] Preparation Example 7
[0090] The carrier was prepared according to the method of Preparation Example 1, except that the particle size of the silicon carbide whisker was 600 nm and the length was 75 μm.
[0091] Preparation Example 8
[0092] The carrier was prepared according to the method of Preparation Example 1, except that the amount of china clay was 70 g, the amount of methyl cellulose was 1 g, the amount of polypropylene was 1 g, and the amount of silica sol was 90 g.
[0093] Preparation Example 9
[0094] The carrier was prepared according to the method of Preparation Example 1, except that china clay and silica sol were replaced by diatomaceous earth.
[0095] Comparative Preparation Example 1
[0096] The carrier was prepared according to the method of Preparation Example 1, except that ordinary spherical silicon carbide powder with a particle size of 50 μm was used instead of silicon carbide whiskers.
[0097] Comparative Preparation Example 2
[0098] The carrier was prepared according to the method of Preparation Example 3, except that ordinary spherical silicon carbide powder with a particle size of 100 μm was used instead of silicon carbide whiskers.
[0099] The carrier structures prepared in the above preparation examples and comparative preparation examples were characterized, and the results are shown in Table 1.
[0100] Table 1
[0101] <![CDATA[Specific surface area (m 2 / g)]]> Thermal conductivity parameters (W / (m·K) Strength (N / mm) Preparation Example 1 1.8 100 30 Preparation Example 2 2.0 112 29 Preparation Example 3 2.4 116 28 Preparation Example 4 2.6 120 27 Preparation Example 5 2.8 124 27 Preparation Example 6 3.2 126 27 Preparation Example 7 3.6 130 27 Preparation Example 8 3.4 128 27 Preparation Example 9 3.6 126 26 Comparative Preparation Example 1 1.0 20 27 Comparative Preparation Example 2 1.2 25 26
[0102] Example 1
[0103] (1) Preparing an active component precursor solution: dissolving 92 g of oxalic acid in 470 mL of water at room temperature, adding 65.6 g of ammonium metavanadate, and adding while stirring until the ammonium metavanadate is dissolved to form a uniform and stable solution; dissolving 27.4 g of ammonium molybdate in 40 mL of water at 40° C., and adding the solution to the above ammonium metavanadate solution, and adding 4.1 g of trisodium phosphate, 1.5 g of diammonium hydrogen phosphate, 1.2 g of nickel nitrate and 1.1 g of indium acetate in sequence while stirring, and mixing to obtain an active component precursor solution.
[0104] (2) Loading of active component precursor: 300 g of the carrier prepared in Preparation Example 1 was placed in a stainless steel drum, and the drum speed was adjusted to 40 rpm / min. When the carrier was heated to 250°C, the carrier temperature was kept constant, and the dark green slurry active component precursor solution was heated to 300°C through a nozzle. The active component precursor solution was then sprayed on the carrier, and the carrier temperature was maintained at 270°C. After spraying, the catalyst precursor was dried at 120°C for 4 h to obtain a catalyst precursor. The content of the active component precursor was 16.4 wt % based on the total weight of the catalyst precursor.
[0105] (3) Activation of catalyst precursor: 150 g of catalyst precursor was placed in an activation furnace. After sealing, the temperature was raised from room temperature to 150 °C at a heating rate of 120 °C / h and maintained for 5 min. The temperature was then raised to 250 °C at a heating rate of 110 °C / h and maintained for 10 min. The temperature was then raised to 350 °C at a heating rate of 100 °C / h and maintained at 350 °C for 20 min. The temperature was then raised to 450 °C at a heating rate of 90 °C / h and maintained at this temperature for 5 h. The temperature was then gradually lowered to room temperature at a rate of 90 °C / h to obtain a catalyst.
[0106] Example 2
[0107] (1) Preparing an active component precursor solution: dissolving 92 g of oxalic acid in 470 mL of water at room temperature, adding 65.6 g of ammonium metavanadate, and adding while stirring until the ammonium metavanadate is dissolved to form a uniform and stable solution; dissolving 30.8 g of ammonium molybdate in 40 mL of water at 40° C., and adding the solution to the above ammonium metavanadate solution, and adding 4.1 g of trisodium phosphate, 1.5 g of diammonium hydrogen phosphate, 1.2 g of nickel nitrate and 1.1 g of indium acetate in sequence while stirring, and mixing to obtain an active component precursor solution.
[0108] (2) Loading of active component precursor: 300 g of the carrier prepared in Preparation Example 2 was placed in a stainless steel drum, and the drum speed was adjusted to 30 rpm / min. When the carrier was heated to 250°C, the carrier temperature was kept constant, and the dark green slurry active component precursor solution was heated to 280°C through a nozzle. The active component precursor solution was then sprayed on the carrier, and the carrier temperature was maintained at 270°C. After spraying, it was dried at 100°C for 8 h to obtain a catalyst precursor. Based on the total weight of the catalyst precursor, the content of the active component precursor was 16.4 wt%.
[0109] (3) Activation of catalyst precursor: 150 g of catalyst precursor was placed in an activation furnace. After sealing, the temperature was raised from room temperature to 150 °C at a heating rate of 80 °C / h and maintained for 20 min. The temperature was then raised to 250 °C at a heating rate of 80 °C / h and maintained for 5 min. The temperature was then raised to 350 °C at a heating rate of 60 °C / h and maintained at 350 °C for 10 min. The temperature was then raised to 420 °C at a heating rate of 60 °C / h and maintained at this temperature for 8 h. The temperature was then gradually lowered to room temperature at a rate of 60 °C / h to obtain a catalyst.
[0110] Example 3
[0111] (1) Preparing an active component precursor solution: dissolving 92 g of oxalic acid in 470 mL of water at room temperature, adding 65.6 g of ammonium metavanadate, and adding while stirring until the ammonium metavanadate is dissolved to form a uniform and stable solution; dissolving 25.8 g of ammonium molybdate in 40 mL of water at 40° C., and adding the solution to the above ammonium metavanadate solution, and adding 3.5 g of trisodium phosphate, 1 g of diammonium hydrogen phosphate, 1.2 g of nickel nitrate and 1.8 g of indium acetate in sequence while stirring, and mixing to obtain an active component precursor solution.
[0112] (2) Loading of active component precursor: 300 g of the carrier prepared in Preparation Example 3 was placed in a stainless steel drum, and the drum speed was adjusted to 20 rpm / min. When the carrier was heated to 250°C, the carrier temperature was kept constant, and the dark green slurry active component precursor solution was heated to 250°C through a nozzle. The active component precursor solution was then sprayed on the carrier, and the carrier temperature was maintained at 270°C. After spraying, the catalyst was dried at 150°C for 2 h to obtain a catalyst. The content of the active component was 16.4 wt % based on the total weight of the catalyst.
[0113] (3) Activation of catalyst precursor: 150 g of catalyst precursor was placed in an activation furnace. After sealing, the temperature was raised from room temperature to 150 °C at a heating rate of 60 °C / h and maintained for 30 min. The temperature was then raised to 250 °C at a heating rate of 50 °C / h and maintained for 30 min. The temperature was then raised to 350 °C at a heating rate of 40 °C / h and maintained at 350 °C for 60 min. The temperature was then raised to 470 °C at a heating rate of 30 °C / h and maintained at this temperature for 10 h. The temperature was then gradually lowered to room temperature at a rate of 40 °C / h to obtain a catalyst.
[0114] Example 4
[0115] The catalyst was prepared according to the method of Example 1, except that 1.1 g of indium acetate was replaced by 0.5 g of antimony trichloride, and the carrier prepared in Preparation Example 4 was used to replace the carrier prepared in Preparation Example 1.
[0116] Example 5
[0117] The catalyst was prepared according to the method of Example 1, except that 1.1 g of indium acetate was replaced by 0.9 g of bismuth nitrate, and the carrier prepared in Preparation Example 5 was used to replace the carrier prepared in Preparation Example 1.
[0118] Example 6
[0119] The catalyst was prepared according to the method of Example 1, except that the carrier prepared in Preparation Example 6 was used to replace the carrier prepared in Preparation Example 1.
[0120] Example 7
[0121] The catalyst was prepared according to the method of Example 1, except that the carrier prepared in Preparation Example 7 was used to replace the carrier prepared in Preparation Example 1.
[0122] Example 8
[0123] The catalyst was prepared according to the method of Example 1, except that the carrier prepared in Preparation Example 8 was used to replace the carrier prepared in Preparation Example 1.
[0124] Example 9
[0125] The catalyst was prepared according to the method of Example 1, except that the carrier prepared in Preparation Example 9 was used to replace the carrier prepared in Preparation Example 1.
[0126] Comparative Example 1
[0127] The catalyst was prepared according to the method of Example 1, except that the carrier prepared in Preparation Example 1 was replaced by the carrier prepared in Comparative Preparation Example 1.
[0128] Comparative Example 2
[0129] The catalyst was prepared according to the method of Example 3, except that the carrier prepared in Comparative Preparation Example 2 was used to replace the carrier prepared in Preparation Example 3.
[0130] Test Case
[0131] The catalysts prepared in the above examples and comparative examples were used for the reaction of benzene oxidation to maleic anhydride, respectively. The reaction was carried out in a 120 mL bubbling molten salt circulation reactor. The reaction conditions included: the molten salt temperature was 350° C., the benzene concentration was 50 Nm 3 , the volume velocity of air is 2200h -1 After running stably for 1 hour, samples were taken for analysis. The analysis results are shown in Table 2.
[0132] Table 2
[0133] Hot spot temperature (℃) Benzene conversion rate (%) Maleic anhydride selectivity (%) Maleic anhydride yield (%) Example 1 457 98.0 78.6 96.8 Example 2 456 98.1 78.4 96.6 Example 3 458 98.4 78.5 97.0 Example 4 458 98.0 77.9 95.9 Example 5 456 97.9 77.7 95.6 Example 6 456 97.9 77.9 95.8 Example 7 465 98.9 74.5 92.6 Example 8 459 98.1 76.1 93.8 Example 9 461 98.8 75.0 93.1 Comparative Example 1 469 99.3 73.6 91.8 Comparative Example 2 471 99.6 73.2 91.6
[0134] From the results in Table 2, it can be seen that the catalyst prepared by the preferred embodiment of the present invention, after being used for the oxidation of benzene to produce maleic anhydride, has a maleic anhydride selectivity higher than 75% and a maleic anhydride yield higher than 92%. And from the hot spot temperatures in Table 2, it can be seen that under the same reaction conditions, the hot spot temperatures of Examples 1-6 using the preferred embodiment of the present invention are in the range of 456-458°C, the maleic anhydride selectivity higher than 77%, and the maleic anhydride yield higher than 95%; while the hot spot temperatures of Examples 7-9 using the non-preferred embodiment of the present invention are in the range of 459-465°C, and the hot spot temperatures of Comparative Examples 1-2 are in the range of 469-471°C, and the maleic anhydride selectivity and maleic anhydride yield are lower than Examples 1-6. It can be seen that the hot spot temperature of the catalyst prepared by the preferred embodiment of the present invention is lower, which is more conducive to the conduction of reaction heat.
[0135] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A catalyst, It is characterized in that The catalyst comprises a carrier and an active component supported on the carrier, wherein the carrier comprises silicon carbide whiskers; The length of the silicon carbide whisker is 2-50 μm, the particle size is 50-500 nm, and the aspect ratio is 20-200; the carrier also contains aluminum oxide and / or silicon dioxide; the content of the silicon carbide whisker is 65-95 g per 100 g of the carrier; The active component includes a first active component and a second active component, the first active component includes at least one of vanadium oxide, molybdenum oxide, sodium oxide, phosphorus oxide and nickel oxide, and the second active component includes at least one of indium oxide, antimony oxide and bismuth oxide.
2. The catalyst according to claim 1, in, The crystal form of the silicon carbide whisker is α-type and / or β-type.
3. The catalyst according to claim 1 or 2, in, The content of the silicon carbide whiskers is 80-94 g per 100 g of the carrier; The active components include the content of each substance in the first active component and the second active component: V 2 O 5 Vanadium oxide, MoO 3 Molybdenum oxide, Na 2 Sodium oxide, calculated as P 2 O 5 The molar ratio of phosphorus oxide calculated as NiO, nickel oxide calculated as NiO and the second active component calculated as metal oxide is 1: (0.2-0.9): (0.001-0.2): (0.005-0.25): (0.0001-0.05): (0.0001-0.05).
4. A method for preparing a catalyst, It is characterized in that The method comprises loading an active component precursor on a carrier and then activating the carrier; wherein the carrier contains silicon carbide whiskers; The length of the silicon carbide whisker is 2-50 μm, the particle size is 50-500 nm, and the aspect ratio is 20-200; the carrier also contains aluminum oxide and / or silicon dioxide; the content of the silicon carbide whisker is 65-95 g per 100 g of the carrier; The active component precursor includes a first active component precursor and a second active component precursor, the first active component precursor includes at least one of a vanadium compound, a molybdenum compound, a sodium compound, a phosphorus compound and a nickel compound, and the second active component precursor includes at least one of an indium compound, an antimony compound and a bismuth compound.
5. The method according to claim 4, in, The crystal form of the silicon carbide whisker is α-type and / or β-type.
6. The method according to claim 4, in, The content of the silicon carbide whisker is 80-94 g per 100 g of the carrier.
7. The method according to claim 4, in, The amount of each substance in the first active component precursor and the second active component precursor is: V 2 O 5 Vanadium compounds, MoO 3 Molybdenum compounds, Na 2 Sodium compounds, calculated as P 2 O 5 The molar ratio of the phosphorus compound calculated as NiO, the nickel compound calculated as NiO and the second active component precursor calculated as metal oxide is 1: (0.2-0.9): (0.001-0.2): (0.005-0.25): (0.0001-0.05): (0.0001-0.05); wherein the indium compound in the second active component precursor is In 2 O 3 Antimony compounds are calculated as Sb 2 O 3 Bi 2 O 3 count; And / or, the vanadium compound is at least one of ammonium metavanadate, vanadium pentoxide and sodium vanadate; And / or, the molybdenum compound is at least one of ammonium molybdate, molybdenum trioxide and calcium molybdate; and / or, the sodium compound is sodium dihydrogen phosphate and / or trisodium phosphate; and / or, the phosphorus compound is at least one of diammonium phosphate, phosphoric acid and phosphorus pentoxide; And / or, the nickel compound is at least one of nickel nitrate, nickel sulfate, nickel chloride and nickel oxide.
8. The method according to claim 4, in, The vanadium compound is ammonium metavanadate.
9. The method according to claim 4, in, The molybdenum compound is ammonium molybdate.
10. The method according to claim 4, in, The sodium compound is trisodium phosphate.
11. The method according to claim 4, in, The nickel compound is nickel nitrate.
12. The method according to any one of claims 4 to 11, in, The carrier is obtained by mixing silicon carbide whiskers, china clay, methyl cellulose, polypropylene and silica sol, and then performing first drying and calcination to obtain the carrier.
13. The method according to claim 12, in, The weight ratio of the silicon carbide whisker, china clay, methyl cellulose, polypropylene and silica sol is 15-45:1-2:0.5-1.5:0.5-1.5:
1.
14. The method according to claim 12, in, The first drying is carried out at a temperature of 100-150° C. and for a time of 6-10 hours.
15. The method according to claim 12, in, The calcination temperature is 800-1200° C. and the calcination time is 3-8 hours.
16. The method according to any one of claims 4 to 11, in, The loading method is: coating the carrier with a solution containing the active component precursor; And / or, the activation conditions include: temperature of 420-470° C. and time of 5-10 h.
17. The method according to claim 16, in, The coating conditions include: a temperature of 250-300°C.
18. A catalyst prepared by the method according to any one of claims 4 to 17.
19. Use of the catalyst according to any one of claims 1 to 3 and 18 in the preparation of maleic anhydride.