A polyurethane pavement material with pavement cooling function

By using polyurethane materials on road surfaces, combining a combination of vegetable oil polyol and polyether polyol and a diisocyanate-modified porous material, the problems of urban heat island effect and environmental pollution are solved, and efficient cooling and durability are achieved.

CN116063026BActive Publication Date: 2024-12-03WANHUA CHEM GRP CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202111298370.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-04
Publication Date
2024-12-03
Estimated Expiration
2041-11-04

AI Technical Summary

Technical Problem

The existing road and pavement materials have strong heat absorption capacity in hot summer environments, resulting in severe urban heat island effects, and traditional cooling methods have problems such as short service life, limited environmental pollution and application range.

Method used

A polyurethane pavement material is used, which contains a polyether and a polyether B-porous material modified polyisocyanate composition. A vegetable oil polyol and polyether polyol are used, and a diisocyanate is modified in component B. Porous materials, by optimizing component ratios and preparation methods, form high-strength, hydrolysis-resistant and aging-resistant pavement materials, significantly reducing pavement temperature.

Benefits of technology

This material can effectively reduce the road surface temperature by 13-15℃, has a long service life, excellent hydrolysis resistance, and is not easily affected by pollutants, avoid environmental pollution, and is suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003337272070000021
    Figure BDA0003337272070000021
  • Figure BDA0003337272070000091
    Figure BDA0003337272070000091
  • Figure BDA0003337272070000101
    Figure BDA0003337272070000101
Patent Text Reader

Abstract

The present invention discloses a polyurethane pavement material with a pavement cooling function. It comprises a component A combined polyether and a component B porous material modified polyisocyanate composition; wherein the component B comprises 8-19% of a heat-insulating material by mass, and based on the mass of the component B, the heat-insulating material is a porous material modified by diisocyanate. The polyurethane pavement material of the present invention has excellent freeze-thaw damage resistance and low-temperature fatigue toughness, can effectively reduce the adsorption of water by the polyurethane material, improve the water damage resistance of the bonding layer and the ability of the polyurethane material to resist long-term hydrolysis. By reducing the absorption, accumulation and barrier effect of solar heat, the pavement temperature can be reduced by up to 15°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pavement materials, and in particular relates to a polyurethane pavement material with a pavement cooling function. Background Art

[0002] With global warming and the gradual increase in the hardening rate of road pavements, the urban heat island phenomenon is becoming more and more obvious, and the quality of urban thermal environment is gradually deteriorating, which has greatly affected the living environment and people's living standards in cities. As the most important surface structure, the road surface has the most significant impact on the urban heat island effect, mainly through the road surface heat conduction, road surface heat radiation and heat convection. The factors affecting the heat island effect of the road mainly include: the heat absorption and storage capacity of the road material, the reflectivity of the road surface, and the thermal conductivity of the road structure. Under the current environment, most of the road pavement structures in my country are asphalt pavements. Due to the black characteristics of asphalt pavements, they have strong heat absorption capacity and the absorption rate of sunlight heat reaches 0.85-0.95. In the hot and high temperature environment in summer, the maximum temperature of the asphalt pavement can reach more than 60°C, which greatly aggravates the urban heat island effect. In view of the serious thermal environment problems existing in urban roads and the increasingly serious phenomenon of urban heat island effect, it is becoming increasingly urgent to develop road pavement materials with cooling effects.

[0003] At present, the method of reducing the road surface temperature reported publicly is mainly to add a heat-reflective coating to the road surface. For example, the publication number CN110437709A "Heat-reflective coating of asphalt pavement and its preparation method" reduces the road surface temperature by adding a heat-reflective coating to the road surface. Although this method can reduce the road surface temperature to a certain extent, it has environmental pollution problems such as short service life of the coating, accumulation and coverage of pollutants such as road dust that reduce the cooling effect of the coating, and volatilization of organic solvents that increase VOC emissions. The publication number CN111170678 A "A castable concrete with polyurethane as a binder and its preparation method" uses a single-component polyurethane binder to prepare a castable concrete, which solves the problem of serious early diseases and short service life of the steel bridge deck pavement layer, but its application field is limited to steel bridge decks, and expensive latent curing agents are used in the preparation process, which is not conducive to large-scale application. The publication number CN110922091 A "Two-component polyurethane composition for concrete modification and its preparation method" uses two-component polyurethane to modify concrete to improve the mechanical properties and mechanical properties of cement concrete materials, solving the problem of poor mechanical properties of polymer-modified cement materials. However, the composite material needs to be pre-treated by water washing, acid washing, etc. during actual application, which greatly reduces the actual use cost and application range. The publication number CN112824474 A "A formaldehyde-free adhesive and a method for preparing composite artificial board using the same, and the prepared composite artificial board" uses modified isocyanate as an adhesive to prepare composite artificial board, solving the problems of the trial period of the adhesive and the water resistance of the board. However, since the curing process of modified isocyanate is wet curing, bubbles will inevitably occur during the curing process, affecting the bonding effect of the adhesive layer. Summary of the invention

[0004] The purpose of the present invention is to provide a polyurethane pavement material with pavement cooling function and a preparation method thereof. The polyurethane pavement material with pavement cooling function has high strength, good bonding performance, excellent hydrolysis stability and aging resistance, long service life, little influence by pollutant accumulation, no environmental pollution and other problems, and can significantly reduce the pavement temperature by 13-15°C.

[0005] In order to achieve the above purpose, the present invention adopts the following technical solutions:

[0006] A polyurethane pavement material with pavement cooling function comprises a component A of a combined polyether and a component B of a porous material modified polyisocyanate composition; wherein the component B comprises 8-19% of a thermal insulation material by mass, and based on the mass of the component B, the thermal insulation material is a porous material modified by diisocyanate.

[0007] The mass ratio of component A to component B of the present invention is 1-2:1, preferably 1.2-1.8:1.

[0008] The component A of the present invention comprises, based on the total mass of the component A:

[0009]

[0010]

[0011] The isocyanate index of the polyurethane pavement material of the present invention is 0.95-1.35, preferably 1.0-1.3.

[0012] The polyol combination of component A of the present invention includes one or more of vegetable oil polyols, polyether polyols, and polyester polyols, and preferably includes the following polyols, based on the total mass of the polyol combination:

[0013] Vegetable oil polyol 1, number average molecular weight of 300-1400, preferably 350-1300, functionality of 2-4, hydroxyl value of 150-300 mgKOH / g, preferably 50-80 wt%, more preferably 53-75 wt%;

[0014] Vegetable oil polyol 2, number average molecular weight 1500-3500, preferably 1600-3400, functionality 2-6, hydroxyl value 50-150 mgKOH / g, preferably 10-40wt%, more preferably 16-37wt%;

[0015] Polyether polyol 1, number average molecular weight 200-400, preferably 220-380, functionality 2-4, hydroxyl value 400-800 mgKOH / g, preferably 1-6wt%, more preferably 1-5wt%;

[0016] Polyether polyol 2, number average molecular weight 400-1000, preferably 450-950, functionality 3-6, hydroxyl value 200-400 mgKOH / g, preferably 1-10 wt%, more preferably 2-8 wt%.

[0017] In the present invention, the vegetable oil polyol 1 in component A is selected from one or more of castor oil, soybean oil, palm oil, sunflower seed oil or its modified products, preferably castor oil and / or its modified products. The castor oil modified product is a castor oil derivative with different hydroxyl values, functionality and molecular weight obtained by alcoholysis and transesterification of ethylene glycol, glycerol, trimethylolpropane and pentaerythritol. Suitable examples include but are not limited to castor oil of Qingdao Tongkai Castor Chemical Co., Ltd., castor oil of Nanjing Jinhaiwei Chemical Industry Co., Ltd., GR-160 and GR-220 of Vertellus Company of the United States, and Uric H-30 and Uric H-854 of Ito Oil Manufacturing Co., Ltd. of Japan.

[0018] In the present invention, the vegetable oil polyol 2 in component A is selected from one or more of castor oil, soybean oil polyol, palm oil, sunflower seed oil or modified products thereof, preferably soybean oil polyol and / or palm oil polyol. Suitable examples include but are not limited to Guangzhou Haierma soybean oil polyol 10100, X-0500 of Cargill Company of the United States, Soyol560 of Beijing Boska Technology Co., Ltd., and PKF 3000 of Maskimi Polyol Company of Malaysia.

[0019] In the present invention, the initiator of the polyether polyol 1 in component A is one or more of glycerol, propylene glycol, ethylene glycol, diethylene glycol, dipropylene glycol, trimethylolpropane, ethylenediamine, triethanolamine, toluenediamine, and sucrose, preferably one or more of glycerol, toluenediamine, triethanolamine, sucrose, and ethylenediamine, more preferably glycerol and or ethylenediamine. Suitable examples include, but are not limited to, A303, A304, and A403 of Wanhua Chemical (Ningbo) Rongwei Polyurethane Co., Ltd.

[0020] In the present invention, the initiator of the polyether polyol 2 in component A is one or more of glycerol, propylene glycol, ethylene glycol, diethylene glycol, dipropylene glycol, trimethylolpropane, ethylenediamine, and triethanolamine, preferably one or more of glycerol, toluenediamine, triethanolamine, sucrose, and trimethylolpropane. Suitable examples include, but are not limited to, A305, A307, A35, A29, and A42-A of Wanhua Chemical (Ningbo) Rongwei Polyurethane Co., Ltd.

[0021] The polymerization monomers of polyether polyol 1 and polyether polyol 2 are one or more of ethylene oxide, propylene oxide and tetrahydrofuran, preferably propylene oxide.

[0022] The chain extender in component A of the present invention includes one or more of alcohol or amine chain extenders. The alcohol chain extender includes but is not limited to 1,4-butanediol, dipropylene glycol, diethylene glycol, 1,6-hexanediol, etc.; the amine chain extender includes but is not limited to 3,3'-dichloro-4,4'-diphenylmethanediamine, 3,5-dimethylthiotoluenediamine, 3,5-diethyltoluenediamine, 4,4'-methylenebis(3-chloro-2,6-diethylaniline), etc. Preferably, one or more of 1,4-butanediol, dipropylene glycol, diethylene glycol, propylene glycol, more preferably 1,4-butanediol and / or propylene glycol. The chain extender can increase the hard segment content of the polyurethane and improve the strength and hardness of the product.

[0023] The wetting and dispersing agent in component A of the present invention is one or more of BYK 9076, BYK 9077, BYK-W961, BYK-W966, BYK-W980, BYK-W969, and BYK-W985, preferably one or more of BYK-980, BYK 9077, BYK-W961, and BYK-W966, and more preferably one or more of BYK-980, BYK 9077, and BYK-W961.

[0024] The catalyst in component A of the present invention is an organic metal catalyst, including one or more of potassium isooctanoate, quaternary ammonium formate, potassium acetate, dibutyltin dilaurate, stannous octoate, dibutyltin diacetate and potassium oleate, preferably dibutyltin dilaurate, and suitable examples include but are not limited to Dabco T12 of Air Products and Chemicals, USA, and Yoke T-12 of Jiangsu Yixing Yake Chemical Co., Ltd.

[0025] The preparation method of component A of the present invention comprises the following steps: according to the proportion, adding a polyol combination and a chain extender into a reaction kettle and stirring for 30-60 minutes, then sequentially adding a wetting dispersant and a catalyst and continuing stirring for 45-70 minutes to obtain component A.

[0026] The B component of the present invention comprises the following composition:

[0027] 8-19wt% of diisocyanate-modified porous material, preferably 10-17wt%;

[0028] Polymethylene polyphenyl isocyanate 81-92wt%, preferably 83-90wt%.

[0029] The diisocyanate described in the present invention is one or more of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate and dicyclohexylmethane diisocyanate.

[0030] The porous material described in the present invention is one or more of nano silicon dioxide, molecular sieve, activated carbon, diatomite, porous silicon oxide and porous aluminum oxide, and its particle size is 0.1-1 nm.

[0031] As a preferred solution, the porous material of the present invention is preferably diatomaceous earth and / or molecular sieve, with a pore size of 0.1-1 nm, preferably 0.2-0.5 nm; a porosity of 75-90%, preferably 80-90%; a specific surface area of ​​60-70 m 2 / g, preferably 62-70m 2 Suitable examples include, but are not limited to, Diatom Pure from Lanrun Environmental Technology and Siliporite NK30 from CECA of Arkema Group, France.

[0032] Preferably, the diisocyanate-modified porous material is diatomaceous earth or molecular sieve modified with diphenylmethane diisocyanate.

[0033] The polymethylene polyphenyl isocyanate described in the present invention includes but is not limited to PM-100, PM-120, PM-200, PM-300, PM-400, PM-2010, PM-2025, PM-6302, and PM-6304 produced by Wanhua Chemical Group Co., Ltd.

[0034] The preparation method of the isocyanate modified porous material of the present invention comprises the following steps: according to the proportion, the porous material is roasted at 300-500°C for 1-1.5h, dispersed in a toluene solution of diisocyanate, heated to 70-90°C and reacted under nitrogen protection for 1-4h, filtered, washed and dried.

[0035] The preparation method of the B component of the present invention comprises the following steps: according to the proportion, polymethylene polyphenyl isocyanate and diisocyanate modified porous material are added into a reaction kettle and stirred for 30-60 minutes to obtain the B component.

[0036] A polyurethane mixture comprises the following components: 18-25 parts by mass of basalt coarse aggregate S10 with a particle size of 10-15 mm, 16-23 parts by mass of basalt coarse aggregate S12 with a particle size of 5-10 mm, 40-58 parts by mass of basalt fine aggregate S15 with a particle size of 0.075-5 mm, 2-12 parts by mass of mineral powder and 3-6 parts by mass of the polyurethane pavement material described in the present invention.

[0037] The preparation method of the polyurethane mixture of the present invention comprises the following steps: according to the proportion, the coarse aggregate S10, the coarse aggregate S12, the fine aggregate S15, the mineral powder and the component A of the polyurethane pavement material of the present invention are stirred for 30-180s, and then the component B of the polyurethane pavement material of the present invention is added and stirred for 30-180s to obtain the polyurethane mixture.

[0038] The positive effects of the present invention are:

[0039] (1) The polyurethane pavement material of the present invention is a pavement bonding material used to replace asphalt. The polyurethane pavement material as a pavement bonding material has the characteristics of high bonding strength, hydrolysis resistance, freeze-thaw resistance, and wear resistance. It can effectively bond aggregates and effectively prevent water from damaging the bonding layer.

[0040] (2) Using polyurethane materials with high thermal resistance instead of asphalt materials effectively reduces the absorption and conduction of heat by the road surface. The pore size of the selected porous material is between 0.2-0.5 nanometers. This special pore size can prevent the isocyanate component from clogging the pores and losing the thermal insulation effect. At the same time, the use of diisocyanate to modify the surface of the porous material not only improves the affinity of the porous material to polyisocyanate to a certain extent, but also effectively improves its dispersibility in the isocyanate component and improves the uniformity of the overall thermal insulation effect of the polyurethane material;

[0041] (3) The vegetable oil polyol 1 and the vegetable oil polyol 2 used in the present invention contain a large number of long-chain fatty groups, which can be inserted into the middle of the polyurethane molecular chain to play a lubricating role, reduce the friction between the polyurethane molecular chains, and at the same time prevent water molecules from hydrolyzing the urethane bonds, thereby giving the polyurethane material better flexibility and hydrolysis resistance; the long-chain fatty groups in the vegetable oil polyol 1 and the vegetable oil polyol 2 do not participate in the reaction with isocyanate, and can be inserted between the polyether segments, thereby reducing the effect of the ether bond on adsorbing water molecules and preventing water molecules from destroying the bonding effect between the polyurethane molecules and the substrate. The ether bond has good low-temperature flexibility due to its low cohesive energy and easy rotation. When the vegetable oil polyol 1 and the vegetable oil polyol 2 and the polyether polyol 1 and the polyether polyol 2 are used simultaneously, the synergistic effect between the vegetable oil polyether polyol and the polyether polyol can be fully exerted, so that the prepared polyurethane material has excellent freeze-thaw damage resistance and low-temperature fatigue toughness;

[0042] (4) The large amount of ester bonds in vegetable oil polyol 1 and vegetable oil polyol 2 can effectively improve the bonding performance between the adhesive and the stone and the thermal oxidation resistance of the adhesive; vegetable oil polyol 1 and vegetable oil polyol 2 contain a large amount of non-polar groups, the presence of these groups can significantly improve the hydrophobicity of the polyol combination; the diisocyanate-modified porous material has the ability to absorb water, and the hydrophobic polyol combination and the porous material with water absorption ability can play a synergistic role when used at the same time, which can effectively reduce the adsorption of water by the polyurethane material, improve the water damage resistance of the adhesive layer and the ability of the polyurethane material to resist long-term hydrolysis. DETAILED DESCRIPTION

[0043] In order to better understand the technical solution of the present invention, the content of the present invention is further described below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0044] Raw material information:

[0045] Vegetable oil polyol 1: Qingdao Tongkai castor oil (molecular weight 929, functionality 2.7, hydroxyl value 163mg KOH / g), GR-160 (molecular weight 928, functionality 2.7, hydroxyl value 164mgKOH / g) from Vertellus, USA;

[0046] Vegetable oil polyol 2: Guangzhou Haierma soybean oil polyol 10100 (molecular weight 2500, hydroxyl value 110mg KOH / g), Beijing Boska Technology Co., Ltd. Soyol560 (molecular weight 1636.25, functionality 3.5, hydroxyl value 120mgKOH / g);

[0047] A310 (comparative example): Tianjin Sanshihua Co., Ltd., molecular weight 1000, functionality 3, hydroxyl value 168 mg KOH / g, glycerol as initiator, PO as repeating unit;

[0048] Polyoxypropylene triol (polyether polyol 1): Wanhua Rongwei A303 (molecular weight 300, functionality 3, hydroxyl value 561 mgKOH / g, glycerol as initiator, PO as repeating unit), Wanhua Rongwei A403 (molecular weight 400, functionality 3, hydroxyl value 420.75 mgKOH / g, glycerol as initiator, PO as repeating unit);

[0049] Polyoxypropylene triol (polyether polyol 2): ​​Wanhua Rongwei A305 (molecular weight 500, functionality 3, hydroxyl value 336.6 mg KOH / g, glycerol as initiator, PO as repeating unit), Wanhua Rongwei A307 (molecular weight 700, functionality 3, hydroxyl value 240.4 mg KOH / g, glycerol as initiator, PO as repeating unit);

[0050] C2004: Wanhua Rongwei, molecular weight 400, functionality 2, hydroxyl value 280.5mg KOH / g, propylene glycol as initiator, PO as repeating unit;

[0051] 1,4-Butanediol: Shanghai Wusong Chemical Plant, molecular weight 90.12, hydroxyl value 1245mg KOH / g;

[0052] 1,2-Propanediol: Huntsman, USA, molecular weight 76.09, 1474.6 mg KOH / g;

[0053] Diatom Pure: Lanrun Environmental Technology;

[0054] 3A molecular sieve: SiliporiteNK30 from CECA of Arkema Group, France;

[0055] BYK9077: BYK Corporation;

[0056] PM-200: Wanhua Chemical PM-200;

[0057] T12: Beijing Zhengheng Chemical Co., Ltd.

[0058] KIT-6 molecular sieve: Klamar (comparative example, pore size 4-10nm)

[0059] 70# asphalt: Shandong Luluguang Road Materials Co., Ltd. (comparative ratio)

[0060] Preparation of isocyanate-modified porous materials:

[0061] In a three-necked flask, 50 parts by mass of MDI-50 and 100 parts by mass of toluene were added and stirred for 5 minutes under nitrogen protection, then 10 parts by mass of the porous material that had been subjected to high-temperature dehydration treatment was added and the mixture was stirred for 15 minutes, heated to 80°C and reacted for 3 hours under nitrogen protection, and after the reaction was completed, naturally cooled to room temperature, filtered, washed, and vacuum dried at 40°C for 12 hours to obtain the isocyanate-modified porous material.

[0062] Example 1

[0063] Preparation of component A: weigh 60 g of castor oil, 24 g of soybean oil 10100, 3 g of R2303, 5 g of R2305, and 4 g of 1,2-propylene glycol in a reactor and stir for 45 min. Then add 3.98 g of BYK9077 and 0.02 g of T12 and continue stirring for 60 min to obtain component A.

[0064] Preparation of component B: weigh 9 g of modified thermal insulation material and 57 g of PM-200 and stir in a reaction kettle for 45 min to obtain component B.

[0065] Preparation of mixture: weigh 305.2g coarse aggregate S10, 278.6g coarse aggregate S12, 653.8g fine aggregate S15, 92.4g mineral powder, 42.2g polyurethane pavement material component A in a mixing pot and stir for 60s, then add 27.8g component B into the mixing pot and stir for 60s to obtain the polyurethane mixture. Prepare the polyurethane mixture rutting board with a rutting thickness of 5cm according to the "Test Specifications for Asphalt and Asphalt Mixtures for Highway Engineering" (JTGE20-2011), and cure it for 24h.

[0066] Rutting plate temperature test: Place the rutting plates in an outdoor environment at the same time and measure the surface temperature of the rutting plates.

[0067] Road performance test: Test relevant performance in accordance with the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTGE20-2011).

[0068] The preparation methods of components A and B, the preparation methods of polyurethane mixtures and the preparation of test pieces in Examples 2-6 and Comparative Examples 1-7 are all based on Example 1.

[0069] Comparative Example 8

[0070] Preparation of mixture: weigh 305.2g of coarse aggregate S10, 278.6g of coarse aggregate S12, and 653.8g of fine aggregate S15 in a mixing pot and heat to 200℃, then add 70g of 70# asphalt heated to 140℃ in the mixing pot and mix for 90s, then add 92.4g of mineral powder and continue mixing for 100s to obtain asphalt mixture. Refer to the "Test Procedure for Asphalt and Asphalt Mixture for Highway Engineering" (JTGE20-2011) to prepare asphalt mixture rutting board with a rutting thickness of 5cm. Make the rutting board and place it in a ventilated place for 24h.

[0071] The addition amount and type of each component of the combined materials of Examples 1-6 and Comparative Examples 1-7 are shown in Table 1 and Table 2 respectively (the addition amount is in parts by mass):

[0072] Table 1 Formulas of various embodiments

[0073]

[0074]

[0075] Table 2 Comparative Examples

[0076] Components 1 2 3 4 5 6 7 castor oil 0 60 0 60 60 60 60 10100 0 0 24 24 24 24 24 A310 84 24 60 0 0 0 0 A303 3 3 3 0 3 0 3 A305 5 5 5 0 0 5 5 C2004 0 0 0 8 5 3 0 1,2-Propanediol 4 4 4 4 4 4 4 BYK9077 3.98 3.98 3.98 3.98 3.98 3.98 3.98 T12 0.02 0.02 0.02 0.02 0.02 0.02 0.02 Modified diatom pure 9 9 9 9 9 9 0 Modified KIT-6 molecular sieve 0 0 0 0 0 0 9 PM-200 57 57 57 57 57 57 57 R 1.01 1.02 1.07 1.15 1.10 1.13 1.09 A:B 1.52 1.52 1.52 1.52 1.52 1.52 1.52

[0077] The temperature and road performance data of Examples 1-6 and Comparative Examples 1-8 are shown in Table 3.

[0078] Table 3 Temperature and road performance data of Examples 1-6 and Comparative Examples 1-8

[0079]

[0080]

[0081] All the polyols used in the comparative example are polyether polyols, and therefore the prepared polyurethane material contains a large number of hydrophilic ether bonds. The presence of these ether bonds greatly enhances the hydrophilicity of the polyurethane pavement material. In addition, the stone itself has a high hydrophilicity. In the presence of stone and a large amount of polyether polyols, water can more easily penetrate into the interface between the polyurethane material and the stone, and destroy the bonding between the polyurethane material and the stone, thereby reducing the residual stability and freeze-thaw splitting strength ratio of the polyurethane pavement material.

[0082] Those skilled in the art will appreciate that, based on the teachings of this specification, some modifications or adjustments may be made to the present invention, and these modifications or adjustments should also be within the scope defined by the claims of the present invention.

Claims

1. A polyurethane pavement material with pavement cooling function, comprising a component A of a combined polyether and a component B of a porous material modified polyisocyanate composition; wherein: The B component contains 8-19% of thermal insulation material by mass, and based on the mass of the B component, the thermal insulation material is a porous material modified by diisocyanate; The mass ratio of component A to component B is 1-2:1; The A component comprises, based on the total mass of the A component: The polyol combination of component A includes one or more of vegetable oil polyol, polyether polyol and polyester polyol; The B component comprises the following components: Diisocyanate modified porous material 8-19wt%, Polymethylene polyphenyl isocyanate 81-92wt%; The preparation method of the diisocyanate-modified porous material comprises the following steps: according to the proportion, the porous material is calcined at 300-500°C for 1-1.5h, dispersed in a toluene solution of diisocyanate, heated to 70-90°C and reacted under nitrogen protection for 1-4h, filtered, washed and dried.

2. The polyurethane pavement material according to claim 1, characterized in that: The mass ratio of component A to component B is 1.2-1.8:

1.

3. The polyurethane pavement material according to claim 1, characterized in that: The A component comprises, based on the total mass of the A component:

4. The polyurethane pavement material according to claim 1, characterized in that: The polyol combination of component A comprises the following polyols, based on the total mass of the polyol combination: Vegetable oil polyol 1, number average molecular weight 300-1400, functionality 2-4, hydroxyl value 150-300 mgKOH / g, 50-80 wt%; Vegetable oil polyol 2, number average molecular weight 1500-3500, functionality 2-6, hydroxyl value 50-150 mgKOH / g, 10-40 wt%; Polyether polyol 1, number average molecular weight 200-400, functionality 2-4, hydroxyl value 400-800 mgKOH / g, 1-6 wt%; Polyether polyol 2, number average molecular weight 400-1000, functionality 3-6, hydroxyl value 200-400 mgKOH / g, 1-10 wt%.

5. The polyurethane pavement material according to claim 1, characterized in that: The polyol combination of component A comprises the following polyols, based on the total mass of the polyol combination: Vegetable oil polyol 1, number average molecular weight 350-1300, functionality 2-4, hydroxyl value 150-300 mgKOH / g, 53-75 wt%; Vegetable oil polyol 2, number average molecular weight 1600-3400, functionality 2-6, hydroxyl value 50-150 mgKOH / g, 16-37 wt%; Polyether polyol 1, number average molecular weight 220-380, functionality 2-4, hydroxyl value 400-800 mgKOH / g, 1-5wt%; Polyether polyol 2, number average molecular weight 450-950, functionality 3-6, hydroxyl value 200-400 mgKOH / g, 2-8 wt%.

6. The polyurethane pavement material according to claim 4, characterized in that: The vegetable oil polyol 1 is selected from one or more of castor oil of Qingdao Tongkai Castor Chemical Co., Ltd., castor oil of Nanjing Jinhaiwei Chemical Industry Co., Ltd., GR-160, GR-220 of Vertellus Company of the United States, Uric H-30, Uric H-854 of Ito Oil Manufacturing Co., Ltd. of Japan; and / or, the vegetable oil polyol 2 is selected from one or more of Guangzhou Haierma soybean oil polyol 10100, X-0500 of Cargill Company of the United States, Soyol560 of Beijing Boska Technology Co., Ltd., and PKF 3000 of Maskimi Polyol Company of Malaysia.

7. The polyurethane pavement material according to claim 4, characterized in that: The polyether polyol 1 is selected from A303, A304, and A403 of Wanhua Chemical (Ningbo) Rongwei Polyurethane Co., Ltd.; and / or, the polyether polyol 2 is selected from one or more of A305, A307, A35, A29, and A42-A of Wanhua Chemical (Ningbo) Rongwei Polyurethane Co., Ltd.

8. The polyurethane pavement material according to claim 1, characterized in that: The B component comprises the following components: Diisocyanate modified porous material 10-17wt%, Polymethylene polyphenyl isocyanate 83-90wt%.

9. The polyurethane pavement material according to claim 1, characterized in that: The porous material is one or more of nano-silicon dioxide, molecular sieve, activated carbon, diatom pure, porous silicon oxide, porous aluminum oxide, and has a pore size of 0.1-1nm, a porosity of 75-90%, and a specific surface area of ​​60-70m 2 / g.

10. The polyurethane pavement material according to claim 1, characterized in that: The porous material is pure diatom and / or molecular sieve, with a pore size of 0.1-1nm, a porosity of 80-90%, and a specific surface area of ​​62-70m 2 / g.

11. The polyurethane pavement material according to claim 10, characterized in that: The pore size is 0.2-0.5 nm.

12. The polyurethane pavement material according to claim 1, characterized in that: The porous material is selected from Diatom Pure of Lanrun Environmental Protection Technology and SiliporiteNK30 of CECA.

Citation Information

Patent Citations

  • Asphalt pavement heat-reflecting coating and preparation method thereof

    CN110437709A

  • Two-component polyurethane composition for concrete modification and preparation method thereof

    CN110922091A

  • Pouring type concrete with polyurethane as binding material and preparation method of pouring type concrete

    CN111170678A

  • Formaldehyde-free adhesive, method for preparing composite artificial board by using formaldehyde-free adhesive and prepared composite artificial board

    CN112824474A

  • Polyurethane combined material, method for preparing polyurethane composite through polyurethane combined material, and application of prepared product

    CN105199071A