High-pressure polyethylene injection molding material and preparation method thereof

By using a specific organic peroxide initiator system to perform multiple polymerizations in the high-pressure polymerization reaction, the problem of insufficient preparation of high-pressure low-density polyethylene injection molding materials was solved, and high-pressure polyethylene injection molding materials suitable for automobile interiors and food packaging were prepared. It achieves the effects of narrow molecular weight distribution and high melting index, simplifies the process and reduces energy consumption.

CN116063603BActive Publication Date: 2024-10-01CHINA PETROLEUM & CHEMICAL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111273330.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-10-01
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

There are few high-pressure low-density polyethylene injection molding plastics produced at home and abroad, and there is a lack of effective preparation processes, which affects the production of automotive interior materials and food packaging box lids.

Method used

By using organic peroxide initiating systems such as tert-butylperoxypivalate and tert-butylperoxy-2-ethylhexanoate in a high-pressure polymerization reaction to perform two polymerization reactions, the melting index of ethylene is adjusted to prepare High-pressure polyethylene injection molding plastic is produced, suitable for automotive interiors and food packaging.

Benefits of technology

The preparation of high-pressure polyethylene injection plastic is realized, which has narrow molecular weight distribution, high melt index and low density, is suitable for the production of injection plastic, simplifies the process and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003329360910000081
    Figure BDA0003329360910000081
Patent Text Reader

Abstract

The present invention relates to a high-pressure polyethylene injection molding compound and a preparation method thereof, the preparation method comprising: S100, allowing ethylene to undergo a first polymerization reaction in the presence of a regulator and a first organic peroxide initiation system, the first organic peroxide initiation system comprising tert-butyl peroxy pivalate and tert-butyl peroxy-2-ethylhexanoate, the reaction temperature being 320-340° C., and the pressure being 255-260 MPa; S200, allowing the first polymerization product containing unreacted ethylene to undergo a second polymerization reaction in the presence of a second organic peroxide initiation system, the second organic peroxide initiation system comprising peroxyacetic acid, tert-butyl peroxy-2-ethylhexanoate and p-menthane hydroperoxide, the reaction temperature being 331-335° C., and the pressure being 240-255 MPa; S300, the second polymerization product is subjected to depressurization, separation and granulation to obtain a high-pressure polyethylene injection molding compound. The preparation method of the present invention is simple, easy to operate, and has low energy consumption. The high-pressure polyethylene injection molding compound has a narrow molecular weight distribution, a high melt index and a low density, and is suitable for the production of injection molding compounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer synthesis, in particular to a high-pressure polyethylene injection molding material and a preparation method thereof. Background Art

[0002] As the global automobile industry has developed rapidly, my country has also listed the automobile industry as a pillar industry. After entering the 21st century, as foreign automobile manufacturers have entered China, my country's car production has made great progress. In order to meet the increasing needs of car drivers, the functional design of automobile interior decoration has become more important, and the expectation for comfort will become higher and higher. The selection and use of interior decoration materials for automobiles, especially small passenger cars, also have a very important impact on the sales and use of automobiles. For this reason, domestic automobile interior parts supporting material manufacturers are also expanding production capacity and improving quality grades at the same time. Using polyethylene special materials for car decoration non-woven fabric backing as raw materials, high-speed extrusion coating process and polyethylene (PE) film backing process are used to coat PE film on non-woven fabrics to form backing to produce automotive interior materials, so that the tensile breaking stress, tensile breaking nominal strain, air tightness and moisture resistance of non-woven fabrics for automotive interiors can be greatly improved. LF2700 produced by Shanghai Petrochemical using the tubular method can be used for car decoration non-woven fabric backing.

[0003] At the same time, people are paying more and more attention to the performance, hygiene, safety and other issues of food packaging, and the requirements for food packaging are getting higher and higher. Polyethylene (PE) has the advantages of good softness, impact resistance, environmental stress cracking resistance, good toughness, high rigidity, heat resistance, and good cold resistance. It is widely used in the field of box covers, including food box covers, storage box covers, sealed box covers, water cup covers, and canned milk powder covers. At present, there are few special materials for box covers in China, and they mainly rely on imported products. In South China, linear products such as South Korea's UJ804, Japan's 2024G, and Guangshihua's DNDA-2020 are the main products. Maoming Petrochemical's full-density polyethylene unit once produced LLDPE box cover materials, but due to the odor problem, it is rarely used in food packaging. The 1# high-pressure unit adopts the patented process technology of Quantum Technology of the United States, which can meet the requirements of producing box cover materials, and the product has a small odor. The development of LDPE multifunctional injection molding special materials on the high-pressure polyethylene unit of Maoming Petrochemical can meet the requirements of the backing adhesive materials for car decoration non-woven fabrics and the injection molding materials for box covers, enriching the product diversity of high-pressure devices and improving the competitiveness of high-pressure device products.

[0004] However, currently, there are few high-pressure low-density polyethylene injection molding materials produced both at home and abroad, and there is still a need to provide high-pressure low-density polyethylene injection molding materials and preparation processes thereof. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a high-pressure polyethylene injection molding material and a preparation method thereof in view of the shortcomings of the prior art. The preparation method of the present invention is simple, easy to operate, and has low energy consumption. The high-pressure polyethylene injection molding material has a narrow molecular weight distribution, a high melt index and a low density, and is suitable for the production of injection molding materials.

[0006] The objectives of the present invention are achieved through the following technical solutions.

[0007] In a first aspect, the present invention provides a method for preparing a high-pressure polyethylene injection molding material, wherein the preparation method comprises the following steps:

[0008] S100, subjecting ethylene to a first polymerization reaction in the presence of a regulator and a first organic peroxide initiation system to obtain a first polymerization product containing unreacted ethylene, wherein the first organic peroxide initiation system comprises tert-butyl peroxypivalate and tert-butyl peroxy-2-ethylhexanoate, and the temperature of the first polymerization reaction is 320-340° C. and the pressure is 250-260 MPa;

[0009] S200, subjecting the first polymerization product containing unreacted ethylene to a second polymerization reaction in the presence of a second organic peroxide initiation system to obtain a second polymerization product, wherein the second organic peroxide initiation system comprises peroxyacetic acid, tert-butyl peroxy-2-ethylhexanoate and para-menthane hydroperoxide, and the temperature of the second polymerization reaction is 331-335° C. and the pressure is 240-255 MPa;

[0010] S300, the second polymerization product is depressurized, separated and granulated to obtain a high-pressure polyethylene injection molding material.

[0011] In the present invention, the melt index of the high-pressure polyethylene can be adjusted by using an adjusting agent.

[0012] According to the preparation method provided by the present invention, wherein the adjusting agent in step S100 is C2-C6 alkane, preferably propane.

[0013] In some embodiments, in step S100, the amount of the regulator is 225±20 ppm based on the weight of the added ethylene.

[0014] According to the preparation method provided by the present invention, in step S100, the first organic peroxide initiation system is added in the form of a solution, and the solvent in the solution of the first organic peroxide initiation system is preferably solvent oil A. Examples of solvent oil A suitable for use in the present invention include, but are not limited to, isoundecane, isododecane, and n-dodecane. In some embodiments, the solvent oil A is selected from at least one of isoundecane and isododecane.

[0015] According to the preparation method provided by the present invention, in step S100, based on the weight of the added ethylene, the amount of tert-butyl peroxypivalate in the first organic peroxide initiation system is 0.5-0.75 weight%, preferably 0.5-0.65 weight%, and more preferably 0.5-0.6 weight%; the amount of tert-butyl peroxy-2-ethylhexanoate is 0.87-1.2 weight%, preferably 0.95-1.0 weight%.

[0016] According to the preparation method provided by the present invention, the time of the first polymerization reaction in step S100 is 8 to 9 seconds.

[0017] According to the preparation method provided by the present invention, the first polymerization reaction in step S100 is carried out in the presence of air. In some embodiments, the output of high-pressure polyethylene injection molding material is 22.8 t / h, and the amount of air used in step S100 is 4-8 m 3 / h. .

[0018] According to the preparation method provided by the present invention, step S100 comprises:

[0019] S101, mixing ethylene with flash ethylene from a primary compressor and / or a secondary compressor, compressing the ethylene to 250-260 MPa via a primary compressor, mixing the ethylene with the circulating material and sending the mixed ethylene to a secondary compressor to be compressed to 265-270 MPa, and adding the regulator from the inlet of the primary compressor;

[0020] S102, sending the mixed gas flow compressed to 265-270 MPa by the secondary compressor into the first reactor, preheating the first reactor, adding the first organic peroxide initiation system from the first initiator injection port, adding air from the inlet of the secondary compressor, heating to 320-340° C., preferably 330-340° C., and conducting a first polymerization reaction at a pressure of 250-260 MPa, preferably 250-255 MPa.

[0021] In some embodiments, in step S102, the first reactor is preheated to 120-160°C, for example, 140°C.

[0022] According to the preparation method provided by the present invention, in step S200, the second organic peroxide initiation system is added in the form of a solution, and the solvent in the solution of the second organic peroxide initiation system is preferably solvent oil B. Examples of solvent oil B suitable for use in the present invention include, but are not limited to, isoundecane, isododecane, isododecane and n-dodecane.

[0023] In some embodiments, based on the weight of the first polymerization reaction product, the amount of acetic acid peroxide in the second organic peroxide initiation system is 0.4 to 0.6 weight %, preferably 0.5 to 0.56 weight %; the amount of tert-butyl peroxy-2-ethylhexanoate is 0.8 to 1.2 weight %, preferably 0.9 to 1.0 weight %; the amount of hydrogen peroxide to menthane is 0.4 to 0.6 weight %, preferably 0.5 to 0.6 weight %.

[0024] According to the preparation method provided by the present invention, the time of the second polymerization reaction in step S200 is 13 to 15 seconds.

[0025] According to the preparation method provided by the present invention, step S200 comprises:

[0026] S201, sending the first polymerization product containing unreacted ethylene into the second reactor, adding the second organic peroxide initiation system from the second initiator injection port, and carrying out the second polymerization reaction at a temperature of 331-335° C. and a pressure of 240-250 MPa.

[0027] According to the preparation method provided by the present invention, step S200 further comprises: before step S201, cooling the first polymerization product containing unreacted ethylene, preferably cooling to 35-40°C.

[0028] According to the preparation method provided by the present invention, step S300 comprises:

[0029] S301, the second polymerization product is cooled to 35-40° C. in the second reactor, the pressure is reduced by the discharge valve at the outlet, and the product is discharged into a high-pressure separator to separate the gas from the product material to obtain ethylene gas and polyethylene product;

[0030] S302, melting the polyethylene product obtained in step S301, and sending it into a low-pressure separator to separate the gas from the product material to obtain ethylene gas and polyethylene product, and granulating them to obtain a high-pressure polyethylene injection molding material.

[0031] According to the preparation method provided by the present invention, the single-pass conversion rate of the preparation method of the present invention is generally 22-25%.

[0032] According to the preparation method provided by the present invention, the preparation method further comprises sending the ethylene gas from the high-pressure separator and / or the low-pressure separator as a circulating material to step S101.

[0033] According to the preparation method provided by the present invention, a tubular high-pressure polymerization process device is used to implement the preparation method of the present invention. The present invention has no special limitation on the tubular high-pressure polymerization process device, and any tubular high-pressure polymerization process device known in the art can be used.

[0034] In a second aspect, the present invention also provides a high-pressure polyethylene injection molding material obtained by the above preparation method.

[0035] According to the high-pressure polyethylene injection plastic provided by the present invention, as measured according to GB / T 3682.1-2000, the melt index of the high-pressure polyethylene injection plastic at a temperature of 190°C and a load of 2.16Kg is 18 to 30g / 10min, preferably 18 to 20g / 10min; and / or the density of the high-pressure polyethylene injection plastic is 0.916 to 0.920g / cm 3 , preferably 0.918~0.920g / cm 3 The molecular weight distribution index (Mw / Mn) of the high-pressure polyethylene injection molding material is 5 to 9, preferably 5 to 6.

[0036] According to the high-pressure polyethylene injection molding material provided by the present invention, the tensile strength of the high-pressure polyethylene injection molding material is greater than 10 MPa, preferably greater than 11 MPa; the tensile fracture strain is greater than 100%, preferably greater than 200%.

[0037] The present invention has the following advantages:

[0038] (1) In the present invention, a high-pressure polyethylene injection molding material is prepared by adjusting the polymerization process, especially the selection of the initiator system, the control of the polymerization pressure and the polymerization temperature, and further controlling the selection and addition amount of the adjusting agent as required, which is of great significance for the research and development of polyethylene special materials;

[0039] (2) The method of the present invention is simple, easy to operate, and has low energy consumption. The single-pass conversion rate of the reaction is 22-25%. The multi-purpose high-pressure polyethylene injection molding compound produced has a narrow molecular weight distribution, a high melt index and a low density, and is suitable for the production of injection molding compounds. DETAILED DESCRIPTION

[0040] The present invention will be further described below in conjunction with specific embodiments, but they do not constitute any limitation to the present invention.

[0041] Example 1

[0042] A high-pressure polyethylene injection molding compound was prepared using a tubular high-pressure polymerization process device according to the following method.

[0043] (1) Ethylene is mixed with flash ethylene from the outlets of the primary compressor and the secondary compressor, compressed to 255 MPa by the primary compressor, mixed with the circulating material and introduced into the inlet of the secondary compressor. Based on the weight of the added ethylene, 225 ppm of propane as a regulator is added from the inlet tank of the primary compressor to obtain a mixed gas stream.

[0044] (2) The secondary compressor compresses the mixed gas flow to 269.1 MPa, and then enters the front part of the first reactor. The first reactor is preheated to 140° C., and the isonadecane solution of the first organic peroxide initiation system is injected from the first initiator injection port, wherein the amount of the organic peroxide tert-butyl peroxy pivalate is 0.5% by weight, and the amount of tert-butyl peroxy-2-ethylhexanoate is 0.95% by weight based on the weight of the added ethylene; the amount of hexene added is 100m 3 / h, 6m3 added from the inlet of the secondary compressor 3 / h of air, the temperature was raised to 330°C, and the first polymerization reaction was carried out at a pressure of 255 MPa. The reaction time was 8 to 9 seconds to obtain a first polymerization reaction product containing unreacted ethylene.

[0045] (3) The first polymerization product containing unreacted ethylene is cooled to 35° C. and fed into a second reactor, and an isoundecane solution of a second organic peroxide initiation system is added from a second initiator injection port, wherein, based on the weight of the first polymerization product, the amount of acetic acid peroxide is 0.5% by weight, the amount of tert-butyl peroxy-2-ethylhexanoate is 0.9% by weight, and the amount of p-menthane hydrogen peroxide is 0.5% by weight. The reaction is reinitiated to carry out a second polymerization reaction to obtain a second polymerization product. The reaction temperature is 331° C., the pressure is 240 MPa, and the reaction time is 13 to 15 seconds.

[0046] (4) The second polymerization product is cooled to 35°C in the second reactor, the pressure is reduced by the discharge valve at the outlet, and the product is discharged into a high-pressure separator to separate the gas from the product material to obtain ethylene gas and polyethylene product. The polyethylene product is melted and sent to a low-pressure separator to separate the gas from the product material to obtain ethylene gas and polyethylene product, which are then granulated to obtain a high-pressure polyethylene injection molding material.

[0047] The single-pass conversion rate of the preparation method of Example 1 is generally 23.6%. The ethylene gas from the high-pressure separator and the low-pressure separator is sent to step (1) as a circulating material.

[0048] Example 2

[0049] The high pressure polyethylene injection molding material was prepared by the same method as in Example 1, except that:

[0050] (a) In step (1), the modifier propane is 215 ppm.

[0051] (b) In step (2), the amount of the organic peroxide tert-butyl peroxypivalate is 0.6% by weight, the amount of tert-butyl peroxy-2-ethylhexanoate is 0.99% by weight, and air is added from the inlet of the secondary compressor. The conditions of the first polymerization reaction are as follows: temperature is 340° C., pressure is 260 MPa, and reaction time is 8 to 9 seconds.

[0052] (c) in step (3), the amount of peroxyacetic acid is 0.56% by weight, the amount of tert-butyl peroxy-2-ethylhexanoate is 0.97% by weight, the amount of hydrogen peroxide to menthane is 0.45% by weight, and the conditions of the second polymerization reaction are as follows: temperature is 331° C., pressure is 245 MPa, and reaction time is 13 to 15 seconds.

[0053] The single-pass conversion rate of the preparation method of Example 2 is generally 23.7%.

[0054] Example 3

[0055] The high pressure polyethylene injection molding material was prepared by the same method as in Example 1, except that:

[0056] (a) In step (1), the modifier propane is 205 ppm.

[0057] (b) In step (2), the amount of the organic peroxide tert-butyl peroxypivalate is 0.62% by weight, the amount of tert-butyl peroxy-2-ethylhexanoate is 1.0% by weight, and air is added from the inlet of the secondary compressor. The conditions of the first polymerization reaction are as follows: temperature is 330° C., pressure is 260 MPa, and reaction time is 8 to 9 seconds.

[0058] (c) in step (3), the amount of peroxyacetic acid is 0.53% by weight, the amount of tert-butyl peroxy-2-ethylhexanoate is 0.97% by weight, the amount of hydrogen peroxide to menthane is 0.60% by weight, and the conditions of the second polymerization reaction are as follows: temperature is 335° C., pressure is 245 MPa, and reaction time is 13 to 15 seconds.

[0059] The single-pass conversion rate of the preparation method of Example 3 is generally 24.6%.

[0060] Example 4

[0061] The high pressure polyethylene injection molding material was prepared by the same method as in Example 1, except that:

[0062] (a) In step (1), the modifier propane is 215 ppm.

[0063] (b) In step (2), the amount of the organic peroxide tert-butyl peroxypivalate is 0.57% by weight, the amount of tert-butyl peroxy-2-ethylhexanoate is 1.05% by weight, and air is added from the inlet of the secondary compressor. The conditions of the first polymerization reaction are as follows: temperature is 330° C., pressure is 260 MPa, and reaction time is 8 to 9 seconds.

[0064] (c) in step (3), the amount of peroxyacetic acid is 0.55 wt %, the amount of tert-butyl peroxy-2-ethylhexanoate is 1.0 wt %, the amount of hydrogen peroxide to menthane is 0.60 wt %, and the conditions of the second polymerization reaction are as follows: temperature is 335° C., pressure is 245 MPa, and reaction time is 13 to 15 seconds.

[0065] The single-pass conversion rate of the preparation method of Example 4 is generally 25.1%.

[0066] Example 5

[0067] The high pressure polyethylene injection molding material was prepared by the same method as in Example 1, except that:

[0068] (a) In step (2), the amount of the organic peroxide tert-butyl peroxypivalate is 0.6% by weight, the amount of tert-butyl peroxy-2-ethylhexanoate is 0.96% by weight, and air is added from the inlet of the secondary compressor. The conditions of the first polymerization reaction are as follows: temperature is 330° C., pressure is 250 MPa, and reaction time is 8-9 seconds.

[0069] (b) in step (3), the amount of peroxyacetic acid is 0.55 wt %, the amount of tert-butyl peroxy-2-ethylhexanoate is 1.0 wt %, the amount of hydrogen peroxide to menthane is 0.60 wt %, and the conditions of the second polymerization reaction are as follows: temperature is 333° C., pressure is 255 MPa, and reaction time is 13 to 15 seconds.

[0070] The single-pass conversion rate of the preparation method of Example 5 is generally 24.8%.

[0071] Example 6

[0072] The high pressure polyethylene injection molding material was prepared by the same method as in Example 1, except that:

[0073] (a) In step (2), the amount of the organic peroxide tert-butyl peroxy pivalate is 0.65% by weight, the amount of the tert-butyl peroxy-2-ethylhexanoate initiator is 0.96% by weight, and air is added from the inlet of the secondary compressor. The conditions of the first polymerization reaction are as follows: temperature 330° C., pressure 250 MPa, and reaction time 8-9 seconds.

[0074] (b) in step (3), the amount of peroxyacetic acid is 0.55 weight %, the amount of tert-butyl peroxy-2-ethylhexanoate is 1.0 weight %, the amount of hydrogen peroxide to menthane is 0.60 weight %, and the conditions of the second polymerization reaction are as follows: reaction temperature is 333° C., pressure is 255 MPa, and reaction time is 13 to 15 seconds.

[0075] The single-pass conversion rate of the preparation method of Example 6 is generally 25.4%.

[0076] Performance Testing

[0077] In the present invention, the following test standards and methods are used to test and standardize high pressure polyethylene injection molding materials.

[0078] Melt mass flow rate: measured according to GB / T 3682.1-2000, conditions: 190°C, 2.16Kg; unit: g / 10min.

[0079] Density: measured according to GB / T 1033.2-2010, condition: temperature 23℃; unit: kg / m 3 .

[0080] Tensile yield strength: measured according to ASTM D638-2010, unit, MPa.

[0081] Elongation at break: measured according to ASTM D638-2010, %.

[0082] Molecular weight distribution (Mw / Mn): Gel permeation chromatography was used, the solvent and mobile phase were 1,2,4-trichlorobenzene (containing 0.025 wt% antioxidant 2,6-dibutyl-p-cresol), the column temperature was 150°C, the flow rate was 1.0 ml / min, and narrow distribution polystyrene standards were used for universal calibration.

[0083] The properties of the high pressure polyethylene injection molding materials prepared in Examples 1 to 6 are shown in Table 1.

[0084] Table 1 Properties of high pressure polyethylene injection molding materials prepared in Examples 1 to 6

[0085]

[0086] As can be seen from Table 1, the high-pressure polyethylene injection molding compound prepared by the preparation method of the present invention has a narrow molecular weight distribution, a high melt index and a low density, and is suitable for the production of injection molding compounds.

[0087] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.

Claims

1. A method for preparing a high-pressure polyethylene injection molding material, wherein: The preparation method comprises the following steps: S100, subjecting ethylene to a first polymerization reaction in the presence of a regulator and a first organic peroxide initiation system to obtain a first polymerization product containing unreacted ethylene, wherein the first organic peroxide initiation system comprises tert-butyl peroxypivalate and tert-butyl peroxy-2-ethylhexanoate, and the temperature of the first polymerization reaction is 320-340° C. and the pressure is 250-260 MPa; S200, subjecting the first polymerization product containing unreacted ethylene to a second polymerization reaction in the presence of a second organic peroxide initiation system to obtain a second polymerization product, wherein the second organic peroxide initiation system comprises peroxyacetic acid, tert-butyl peroxy-2-ethylhexanoate and para-menthane hydroperoxide, and the temperature of the second polymerization reaction is 331-335° C. and the pressure is 240-255 MPa; S300, the second polymerization product is subjected to pressure reduction, separation and granulation to obtain a high-pressure polyethylene injection molding material; The adjusting agent in step S100 is propane; based on the weight of the added ethylene, the amount of the adjusting agent in step S100 is 225±20 ppm; In step S100, the first organic peroxide initiation system is added in the form of a solution; In step S200, the second organic peroxide initiation system is added in the form of a solution.

2. The preparation method according to claim 1, characterized in that: In step S100, the solvent in the solution of the first organic peroxide initiation system is solvent oil A, and the solvent oil A is selected from at least one of isoundecane, isododecane and n-dodecane.

3. The preparation method according to claim 2, characterized in that: The solvent oil A is at least one of isoundecane and isododecane.

4. The preparation method according to claim 1, characterized in that: In step S100, based on the weight of the added ethylene, the amount of tert-butyl peroxypivalate in the first organic peroxide initiation system is 0.5-0.75 wt %; the amount of tert-butyl peroxy-2-ethylhexanoate is 0.87-1.2 wt %.

5. The preparation method according to claim 4, characterized in that: In step S100, based on the weight of the added ethylene, the amount of tert-butyl peroxypivalate in the first organic peroxide initiation system is 0.5 to 0.65 weight %.

6. The preparation method according to claim 5, characterized in that: In step S100, based on the weight of the added ethylene, the amount of tert-butyl peroxypivalate in the first organic peroxide initiation system is 0.5-0.6 wt%.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The first polymerization reaction in step S100 lasts for 8 to 9 seconds and is carried out in the presence of air. Based on the output of high-pressure polyethylene injection molding material of 22.8 t / h, the amount of air used in step S100 is 4 to 8 m 3 / h.

8. The preparation method according to any one of claims 1 to 6, characterized in that: Step S100 includes: S101, mixing ethylene with flash ethylene from the primary compressor and / or the secondary compressor, compressing the ethylene to 250-260 MPa via the primary compressor, mixing the ethylene with the circulating material and sending the mixed ethylene to the secondary compressor to be compressed to 265-270 MPa, and adding the adjusting agent from the inlet of the primary compressor; S102, sending the mixed gas flow compressed to 265-270 MPa by the secondary compressor into the first reactor, preheating the first reactor, adding the first organic peroxide initiation system from the first initiator injection port, adding air from the inlet of the secondary compressor, raising the temperature to 320-340° C., and conducting the first polymerization reaction at a pressure of 250-260 MPa.

9. The preparation method according to claim 8, characterized in that: Step S102, adding air from the inlet of the secondary compressor, raising the temperature to 330-340° C., and performing the first polymerization reaction at a pressure of 250-255 MPa.

10. The preparation method according to any one of claims 1 to 6, characterized in that The solvent in the solution of the second organic peroxide initiation system in step S200 is solvent oil B, and the solvent oil B is selected from at least one of isoundecane, isododecane, isododecane and n-dodecane.

11. The preparation method according to claim 10, characterized in that Based on the weight of the first polymerization product, the amount of peroxyacetic acid in the solution of the second organic peroxide initiation system is 0.4-0.6 weight %; the amount of tert-butyl peroxy-2-ethylhexanoate is 0.8-1.2 weight %; and the amount of hydrogen peroxide to menthane is 0.4-0.6 weight %.

12. The preparation method according to claim 11, characterized in that: Based on the weight of the first polymerization product, the amount of peroxyacetic acid in the solution of the second organic peroxide initiation system is 0.5-0.56 weight %; the amount of tert-butyl peroxy-2-ethylhexanoate is 0.9-1.0 weight %; and the amount of hydrogen peroxide to menthane is 0.5-0.6 weight %.

13. The preparation method according to any one of claims 1 to 6, characterized in that: Step S200 includes: S201, feeding the first polymerization product containing unreacted ethylene into a second reactor, adding a second organic peroxide initiation system from a second initiator injection port, and performing a second polymerization reaction at a temperature of 331-335° C. and a pressure of 240-250 MPa.

14. The preparation method according to claim 13, characterized in that: Step S200 further includes: before step S201, cooling the first polymerization product containing unreacted ethylene.

15. The preparation method according to claim 14, characterized in that: Cool to 35-40℃.

16. The preparation method according to claim 13, characterized in that: The duration of the second polymerization reaction in step S200 is 13 to 15 seconds.

17. The preparation method according to any one of claims 1 to 6, characterized in that: Step S300 includes: S301, cooling the second polymerization product to 35-40° C. in the second reactor, reducing the pressure through a discharge valve at the outlet, and discharging the product into a high-pressure separator to separate gas from product materials to obtain ethylene gas and polyethylene products; S302, melting the polyethylene product obtained in step S301, and sending it into a low-pressure separator to separate the gas from the product material to obtain ethylene gas and polyethylene product, and granulating them to obtain a high-pressure polyethylene injection molding material.

18. High-pressure polyethylene injection molding material obtained by the preparation method according to any one of claims 1 to 17.

19. The high-pressure polyethylene injection molding material according to claim 18, characterized in that: According to GB / T3682.1-2000, the melt index of the high-pressure polyethylene injection material at a temperature of 190°C and a load of 2.16Kg is 18-30g / 10min; and / or the density of the high-pressure polyethylene injection material is 0.916-0.920g / cm 3 The molecular weight distribution index (Mw / Mn) of the high-pressure polyethylene injection molding material is 5 to 9.

20. The high-pressure polyethylene injection molding material according to claim 19, characterized in that: According to GB / T3682.1-2000, the melt index of the high-pressure polyethylene injection material at a temperature of 190°C and a load of 2.16Kg is 18-20g / 10min; and / or the density of the high-pressure polyethylene injection material is 0.918-0.920g / cm 3 ; The molecular weight distribution index (Mw / Mn) of the high-pressure polyethylene injection molding material is 5 to 6.