Method for treating nickel salt and acid by membrane method in hydrometallurgy and positive electrode material of battery

Through the combined technology of diffusion dialysis membrane system and electrodialysis membrane treatment equipment, efficient physical separation of nickel sulfate is achieved, which solves the problems of chemical agent use and wastewater generation in traditional processes, obtains high-purity nickel salts and acids, and improves safety. and environmental protection.

CN116065033BActive Publication Date: 2024-10-15GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310001655.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-03
Publication Date
2024-10-15
Estimated Expiration
2043-01-03

AI Technical Summary

Technical Problem

The traditional hydrometallurgical process requires the addition of chemical agents when preparing nickel sulfate, resulting in high production costs and potential safety hazards. The recovery rate of acid is low, and a large amount of wastewater is generated, which affects environmental protection.

Method used

The diffusion dialysis membrane system is used to physically separate the nickel-containing precipitation liquid, and the electrodialysis membrane treatment equipment is used to concentrate the dilute acid solution to achieve efficient separation of nickel salts and acids, avoiding the use of chemicals and ensuring the safety of the process. safety and environmental protection.

Benefits of technology

High-purity nickel salt and acid are obtained at room temperature, with a separation rate of 95% and a nickel ion interception rate of 98%, which reduces production costs, avoids the generation of waste water, and improves acid recovery and utilization. It is suitable for nickel hydrogen, nickel Preparation of cadmium batteries and nickel-cobalt hydroxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116065033B_ABST
    Figure CN116065033B_ABST
Patent Text Reader

Abstract

The present application provides a method for treating nickel salts and acids by a hydrometallurgical membrane method and a positive electrode material for a battery. The above-mentioned hydrometallurgical membrane method for treating nickel salts and acids comprises the following steps: obtaining a nickel-containing precipitated liquid; treating the nickel-containing precipitated liquid by a diffusion dialysis membrane system to obtain a nickel salt concentrate and a dilute acid solution; evaporating and concentrating the nickel salt concentrate to obtain a nickel salt product; concentrating the dilute acid solution by an electrodialysis membrane treatment device to obtain an acid product. Since the method uses a diffusion dialysis membrane system to treat the nickel-containing precipitated liquid, it belongs to physical separation, and a nickel salt with a good structural morphology and high purity can be obtained at room temperature, that is, the separation rate of the acid reaches 95%, and the interception rate of nickel ions reaches 98%, so that the obtained nickel salt can be directly used in the preparation of nickel-hydrogen, nickel-cadmium batteries and nickel-cobalt hydroxides, which is not only simple and safe to operate, but also low in cost, and the whole process does not produce wastewater, which is more conducive to environmental protection and energy saving.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrometallurgy, in particular to a method for treating nickel salt and acid by membrane method in hydrometallurgy and a positive electrode material for a battery. Background Art

[0002] Nickel sulfate is mainly used in the electroplating industry and the battery industry. It is the main nickel salt for electroplating nickel and chemical nickel. In recent years, due to the substantial increase in demand for positive electrode materials for power batteries and the impact of high nickel content in batteries, the demand for nickel sulfate has shown explosive growth. Therefore, the resources of nickel sulfate will become another problem restricting the development of battery materials and recycling business.

[0003] At present, nickel sulfate is obtained from nickel ore hydrometallurgy. In actual industrial applications, sulfuric acid is usually added first to leach nickel salts and acids, and then nickel beans / nickel powder, sulfuric acid, and hydrogen peroxide are added to form a slurry. The slurry is then subjected to solid-liquid separation to obtain a nickel sulfate solution. Finally, the nickel sulfate solution is evaporated and concentrated to obtain a nickel salt product.

[0004] It can be seen that the traditional process uses chemical reactions to prepare nickel sulfate, that is, it is necessary to add three chemical agents, nickel beans / nickel powder, sulfuric acid, and hydrogen peroxide, to increase the concentration of nickel sulfate in the slurry. This not only results in a high production cost of nickel sulfate, but also sulfuric acid and hydrogen peroxide have strong oxidizing properties, which can easily cause safety accidents if not operated properly. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for physically separating nickel sulfate and treating nickel salts and acids by a hydrometallurgical membrane method which is safe and environmentally friendly, and a battery positive electrode material.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] A method for treating nickel salt and acid by a hydrometallurgical membrane method, comprising the following steps:

[0008] Obtaining a nickel-containing precipitate solution;

[0009] The nickel-containing precipitated liquid is treated by a diffusion dialysis membrane system to obtain a nickel salt concentrate and a dilute acid solution;

[0010] The nickel salt concentrate is evaporated and concentrated to obtain a nickel salt product;

[0011] The dilute acid solution is concentrated by electrodialysis membrane treatment equipment to obtain an acid product.

[0012] In some other embodiments, when the nickel-containing precipitated liquid is treated by a diffusion dialysis membrane system, the membrane entry requirements are: suspended solids <1.0 mg / L, H +Concentration ≤6mol / L, total nickel salt concentration: total acid concentration ≤1:10, COD<200mg / L, operating temperature: 15℃~45℃.

[0013] In some other embodiments, when the nickel-containing precipitated solution is treated by a diffusion dialysis membrane system, the dialysis coefficient is 10*10 -7 m / s~20*10 -7 m / s, acid salt separation factor 40.

[0014] In some other embodiments, when the nickel-containing precipitated liquid is treated by a diffusion dialysis membrane system, the pH of the nickel-containing precipitated liquid is 1.5-3.0.

[0015] In some other embodiments, the electrodialysis membrane treatment equipment has an ion exchange capacity of 0.8 mol / Kg to 1.5 mol / Kg, a migration number > 0.97, and a membrane resistance of 2.8 Ωm / cm 2 ~3.5Ωm / cm 2 Concentrated under the conditions.

[0016] In some other embodiments, the step of obtaining the nickel-containing precipitated liquid includes the following specific steps:

[0017] Obtaining nickel-containing ore;

[0018] Crushing and screening the nickel-containing ore to obtain nickel-containing ore particles;

[0019] Leaching the nickel-containing ore particles with an acid solution to obtain a nickel-containing mixed solution;

[0020] The nickel-containing mixed solution is filtered to remove impurities and obtain a nickel-containing precipitated solution.

[0021] In some other embodiments, after the step of concentrating the dilute acid solution by electrodialysis membrane treatment equipment to obtain an acid product, the following steps are also included:

[0022] The acid product is compounded with concentrated acid to obtain the acid solution described in the above embodiment.

[0023] In some other embodiments, the concentration of the acid product is ≥120 g / L.

[0024] In some other embodiments, the step of evaporating and concentrating the nickel salt concentrate includes the following specific steps:

[0025] The nickel salt concentrate is pumped into the nickel salt MVR evaporation concentration equipment for evaporation concentration and impurity removal.

[0026] A battery positive electrode material comprises the nickel salt product prepared by treating a nickel salt and an acid by a hydrometallurgical membrane method as described in at least any one of the above embodiments.

[0027] Compared with the prior art, the present invention has at least the following advantages:

[0028] The above-mentioned hydrometallurgical membrane method for treating nickel salts and acids, since this method uses a diffusion dialysis membrane system to treat the nickel-containing precipitate liquid, belongs to physical separation, and can obtain nickel salts with better structure and higher purity at room temperature, that is, the acid separation rate reaches 95%, and the nickel ion interception rate reaches 98%, so that the obtained nickel salt can be directly used in the preparation of nickel-hydrogen, nickel-cadmium batteries and nickel-cobalt hydroxide. Compared with the traditional treatment process, since the diffusion dialysis membrane system does not need to add chemicals, it is not only simple and safe to operate, but also low in cost. At the same time, the dilute acid solution is concentrated in conjunction with the electrodialysis membrane treatment equipment to ensure that the H in the diffusion dialysis membrane + It can be maintained within a certain concentration to ensure that the diffusion dialysis membrane system can continuously circulate and operate, and the entire process does not generate wastewater, which is more conducive to environmental protection and energy saving. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0030] Figure 1 A flow chart of a method for treating nickel salt and acid by membrane method in hydrometallurgy according to one embodiment of the present invention;

[0031] Figure 2 The present invention is an overall flow chart of a method for treating nickel salt and acid by membrane method in hydrometallurgy according to one embodiment of the present invention. DETAILED DESCRIPTION

[0032] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0033] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.

[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to suppress the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0035] The present application provides a method for treating nickel salts and acids by a membrane method in hydrometallurgy, comprising the following steps: obtaining a nickel-containing precipitated liquid; treating the nickel-containing precipitated liquid by a diffusion dialysis membrane system to obtain a nickel salt concentrate and a dilute acid solution; evaporating and concentrating the nickel salt concentrate to obtain a nickel salt product; and concentrating the dilute acid solution by an electrodialysis membrane treatment device to obtain an acid product.

[0036] The above-mentioned hydrometallurgical membrane method for treating nickel salts and acids, since this method uses a diffusion dialysis membrane system to treat the nickel-containing precipitate liquid, belongs to physical separation, and can obtain nickel salts with better structure and higher purity at room temperature, that is, the acid separation rate reaches 95%, and the nickel ion interception rate reaches 98%, so that the obtained nickel salt can be directly used in the preparation of nickel-hydrogen, nickel-cadmium batteries and nickel-cobalt hydroxide. Compared with the traditional treatment process, since the diffusion dialysis membrane system does not need to add chemicals, it is not only simple and safe to operate, but also low in cost. At the same time, the dilute acid solution is concentrated in conjunction with the electrodialysis membrane treatment equipment to ensure that the H in the diffusion dialysis membrane + It can be maintained within a certain concentration to ensure that the diffusion dialysis membrane system can continuously circulate and operate, and the entire process does not generate wastewater, which is more conducive to environmental protection and energy saving.

[0037] See also Figure 1 In order to better understand the technical solution and beneficial effects of the present application, the present application is further described in detail below in conjunction with specific examples. A method for treating nickel salt and acid by a hydrometallurgical membrane method in one embodiment includes some or all of the following steps:

[0038] S100, obtaining a nickel-containing precipitate solution.

[0039] See also Figure 2 In some other embodiments, the step of obtaining the nickel-containing precipitated liquid includes the following specific steps:

[0040] Obtain nickel-containing ore; crush and screen the nickel-containing ore to obtain nickel-containing ore particles; use an acid solution to leaching the nickel-containing ore particles to obtain a nickel-containing mixed solution; remove impurities and filter the nickel-containing mixed solution to obtain a nickel-containing precipitated solution.

[0041] It can be understood that the nickel-containing ore is crushed and screened to obtain nickel-containing ore particles with smaller particle size, so that the nickel-containing ore particles can be better leached by the acid solution. Further, the nickel-containing ore is crushed by a coarse crushing device, the crushed nickel-containing ore is crushed, and the crushed nickel-containing ore is screened to obtain nickel-containing ore particles with smaller particle size. Further, the mesh number of the sieve for the screening operation is less than 20; then the nickel-containing ore particles are placed in a reaction tank, and an excess of acid solution is added for leaching treatment to obtain a nickel-containing mixed solution. Further, in order to ensure that the obtained nickel-containing precipitated liquid can be well diffused and dialyzed in the diffusion dialysis membrane system, therefore, in the present application, by controlling the addition of excess acid solution and controlling pH<1.0; in this way, on the one hand, the leaching rate of the nickel-containing ore particles can be improved, and on the other hand, the concentration of the leaching solution of the subsequent acid solution can be ensured to be ≥70g / L, which is conducive to the subsequent diffusion dialysis of the nickel-containing precipitated liquid in the diffusion dialysis membrane system. Furthermore, the ratio of the nickel salt to the acid is 1: (4-5) to ensure that the added acid is excessive to ensure that the excess acid can better leach the nickel salt. Furthermore, in order to improve the leaching rate of the nickel-containing ore particles, in another embodiment, the nickel-containing mixed solution is also subjected to a filter press operation to obtain a nickel-containing leaching solution and nickel-containing ore particles, and the nickel-containing ore particles continue to be leached. When the sulfuric acid concentration of the nickel-containing leaching solution is ≥70g / L, the next round of impurity removal and filtration is entered.

[0042] Then, the nickel-containing leaching solution is filtered to remove impurities. Specifically, nickel carbonate is added to adjust the pH to 2.0, and an impurity remover is added to precipitate impurities to remove impurities such as chromium and iron, so as to prevent impurities from entering the diffusion dialysis membrane system and affecting the effect of diffusion dialysis. Furthermore, the impurity remover includes 1L (Fe: 1g / L) mixed solution, 8mL7.8%H2O2, and 2.5mL85%H3PO4. The nickel-containing leaching solution after impurities removal is aged, and the aged nickel-containing leaching solution is pumped into a filter press for solid-liquid separation. The filtrate obtained is the nickel-containing precipitated liquid, and the nickel-containing precipitated liquid is pumped into the diffusion dialysis membrane treatment system only when the acid concentration in the nickel-containing precipitated liquid is ≥70g / L, so as to ensure that the nickel-containing precipitated liquid can be well diffused and dialyzed in the diffusion dialysis membrane system.

[0043] In some other embodiments, the nickel salt includes at least one of nickel sulfate, nickel chloride and nickel hydroxide. In a preferred embodiment, the nickel salt is nickel sulfate.

[0044] In some other embodiments, the acid is at least one of sulfuric acid, hydrochloric acid and nitric acid. In a preferred embodiment, the acid is sulfuric acid.

[0045] In this embodiment, the nickel-containing precipitated liquid is mainly composed of a mixed solution of nickel sulfate and sulfuric acid. When the concentration of sulfuric acid in the nickel-containing precipitated liquid is ≥70 g / L, the nickel-containing precipitated liquid enters the diffusion dialysis membrane system for treatment.

[0046] S200, treating the nickel-containing precipitated liquid through a diffusion dialysis membrane system to obtain a nickel salt concentrate and a dilute acid solution.

[0047] It can be understood that since the diffusion dialysis membrane system is an ion migration process, for example, the acid is H2SO4 2 , the nickel salt is nickel sulfate, driven by the concentration difference, SO4 2- When SO4 2- When migrating to the receiving liquid side, H + and Ni 2+ In the past, but because H + The ionic radius is smaller than Ni 2+ Ionic radius, H + With SO4 2- Dialysis has passed, and most of the Ni 2+ is blocked, while the OH in the recovery chamber - The ion concentration is higher than that in the feed liquid chamber, OH - Ions pass through the anion membrane into the material liquid chamber and interact with H + Ions combine to form water to achieve the separation of nickel salt and acid, which is a physical separation. Nickel salt with better structure and higher purity can be obtained at room temperature, that is, the acid separation rate reaches 95%, and the nickel ion interception rate reaches 98%, so that the obtained nickel salt can be directly used in the preparation of nickel-hydrogen, nickel-cadmium batteries and nickel-cobalt hydroxide. Compared with traditional treatment processes, since the diffusion dialysis membrane system does not require the addition of chemicals, it is not only simple and safe to operate, but also low in cost.

[0048] In order to ensure that the diffusion dialysis membrane system can well penetrate the nickel-containing precipitated liquid, in some other embodiments, when the nickel-containing precipitated liquid is treated by the diffusion dialysis membrane system, the pH of the nickel-containing precipitated liquid is 1.5-3.0, and at the same time, the membrane entry requirements are: suspended solids <1.0 mg / L, H + Concentration ≤ 6 mol / L, total nickel salt concentration: total acid concentration ≤ 1:10, COD (Chemical Oxygen Demand) < 200 mg / L, operating temperature: 15°C ~ 45°C, and dialysis coefficient 10*10-7 m / s~20*10 -7 m / s, acid salt separation factor 40, thus ensuring that the nickel-containing precipitated liquid can quickly diffuse and permeate in the diffusion dialysis membrane system.

[0049] In order to ensure that the nickel-containing precipitated liquid can be evenly diffused in the diffusion dialysis membrane system, in some other embodiments, the diffusion dialysis membrane system includes a feed liquid and a receiving liquid, and the feed liquid and the receiving liquid flow in countercurrent. The feed liquid is the nickel-containing precipitated liquid, and the receiving liquid is fresh water, wherein the fresh water includes fresh water and distilled water produced by the post-process electrodialysis membrane system, and the flow ratio of the nickel-containing precipitated liquid to the receiving liquid is 1: (0.85~0.95).

[0050] It can be understood that since the fresh water and distilled water receiving the receiving solution in the diffusion dialysis membrane system contain weak acid, that is, they contain trace amounts of H + , so that the added receiving liquid can, on the one hand, increase the diffusion rate of the liquid in the diffusion dialysis membrane system, thereby increasing the separation rate of the nickel salt concentrate and the dilute acid solution, and on the other hand, can effectively reduce the amount of the added receiving liquid. Compared with the traditional diffusion dialysis membrane system, conventional water is usually selected as the receiving liquid, and the flow ratio of the nickel-containing precipitated liquid to the receiving liquid needs to be controlled to be 1:1. Compared with the flow ratio of the nickel-containing precipitated liquid to the receiving liquid of the present application of 1:(0.85~0.95), the unit addition amount of the traditional receiving liquid is relatively high, which not only increases the usage of the traditional receiving liquid, thereby increasing the cost, but also generates a large amount of wastewater, which is not conducive to environmental protection, and also reduces the separation rate of the nickel salt concentrate and the dilute acid solution, resulting in low production efficiency. Therefore, the present application uses fresh water and distilled water as the receiving liquid of the diffusion dialysis membrane system, which can reduce the use of the receiving liquid and reduce the cost on the one hand, and improve the recycling rate of the acid on the other hand, so that the entire production process does not produce wastewater, which is more conducive to energy conservation and environmental protection, and on the other hand, it also increases the separation speed of the nickel salt concentrate and the dilute acid solution, thereby improving production efficiency. In a preferred embodiment, the flow ratio of the nickel-containing precipitated liquid to the receiving liquid is 1:0.95.

[0051] Furthermore, the concentration of the receiving solution is 50 mg / L to 200 mg / L, so that the H + The concentration is relatively suitable to ensure that the H + The concentration of Ni 2+ The concentration can maintain a relatively good diffusion concentration, thereby ensuring that when the nickel-containing precipitate is diffused, Ni 2+ No crystallization will occur, ensuring a high separation rate between the nickel salt and the dilute acid solution, that is, the acid separation rate is ≥95% and the nickel ion interception rate is ≥98%.

[0052] S300, evaporating and concentrating the nickel salt concentrate to obtain a nickel salt product.

[0053] In this embodiment, the step of evaporating and concentrating the nickel salt concentrate includes the following specific steps: pumping the nickel salt concentrate into a nickel salt MVR (mechanical vapor recompression, industrial wastewater MVR evaporator) evaporation and concentration equipment for evaporation, concentration and impurity removal to obtain a nickel salt product and a concentrated mother liquor.

[0054] S400, concentrating the dilute acid solution through an electrodialysis membrane treatment device to obtain an acid product.

[0055] It can be understood that since the electrodialysis membrane treatment equipment performs an acid concentration method on the dilute acid solution, the electrodialysis membrane treatment equipment can concentrate the dilute acid solution diffused and separated by the diffusion dialysis membrane system, thereby ensuring that the H + The concentration of Ni 2+ The concentration can be maintained at a good concentration to ensure that the newly pumped nickel-containing precipitated liquid can continuously undergo diffusion dialysis in the diffusion dialysis membrane system, thereby ensuring that the diffusion dialysis membrane system can continuously circulate, and the dilute acid solution after passing through the electrodialysis membrane treatment equipment can obtain acid products and fresh water. In order to improve the recovery rate of the acid in the method for treating nickel salts and acids by membrane method in hydrometallurgy of the present application, the present application uses the acid product and concentrated acid to obtain an acid solution to leach the nickel-containing ore particles. At the same time, the fresh water can be circulated back to the diffusion dialysis membrane system. Since the fresh water contains trace amounts of H + , so that the added fresh water can, on the one hand, increase the diffusion rate of the liquid in the diffusion dialysis membrane system, thereby improving the separation rate of the nickel salt concentrate and the dilute acid solution, and on the other hand, can effectively reduce the amount of receiving liquid added, which not only improves the recovery rate of the acid, but also does not generate wastewater, saving energy and being environmentally friendly. In other words, the fresh water containing weak acid generated by the electrodialysis membrane treatment equipment does not need further treatment and can be directly reused in the diffusion dialysis system, without wasting water resources and requiring no secondary equipment for treatment and reuse, thereby reducing costs and equipment investment.

[0056] Furthermore, in some other embodiments, the electrodialysis membrane treatment equipment is a homogeneous electrodialysis membrane treatment equipment, so as to ensure that a high acid recovery rate is obtained while also taking into account fresh water with a moderate weak acid concentration, so as to ensure that the fresh water with a moderate weak acid concentration can be better circulated back into the diffusion dialysis system.

[0057] Furthermore, in some other embodiments, the electrodialysis membrane treatment equipment is concentrated under the conditions of ion exchange capacity of 0.8mol / Kg~1.5mol / Kg, migration number>0.97, and membrane resistance of 2.8Ωm / cm2~3.5Ωm / cm2 to ensure that acid products and fresh water can be obtained, so as to better recover the acid products to the step of leaching the nickel-containing ore particles and recover the fresh water to the diffusion dialysis membrane system. In some other embodiments, the concentration of the acid product is ≥120g / L. In some other embodiments, the fresh water contains H + The concentration is 50mg / L~200mg / L.

[0058] It should be noted that when fresh water contains H + When the concentration is less than 50 mg / L, the acid content in the dilute acid solution is relatively small. If the dilute acid solution is continuously ionized and concentrated, the acid crystals will increase, which will easily cause scaling of the membrane of the electrodialysis membrane treatment equipment, thereby affecting the normal operation of the electrodialysis membrane treatment equipment. When the weak acid concentration of fresh water is greater than 200 mg / L, when the fresh water greater than 200 mg / L is reused in the diffusion dialysis membrane system, it will cause H + The concentration increases, thus affecting Ni 2+ The diffusion of nickel-containing liquid acid reduces the separation rate of nickel-containing precipitation under the same diffusion dialysis conditions, thereby reducing the acid recovery rate. Therefore, the present application sets the concentration of fresh water to 50mg / L~200mg / L, which can avoid scaling of the membrane of the electrodialysis membrane treatment equipment on the one hand, thereby extending the service life of the electrodialysis membrane treatment equipment, and on the other hand, ensure that the H of the fresh water recycled to the diffusion dialysis system is + The concentration is relatively suitable to ensure that the H + with Ni 2+ The concentration is relatively suitable, thereby ensuring that nickel salts are not prone to crystallization during diffusion dialysis, so as to improve the recovery rate of nickel salts while also taking into account a higher acid separation rate, that is, the acid separation rate is ≥85%, the nickel ion interception rate is ≥95%, and the diffusion rate of the liquid in the diffusion dialysis membrane system is increased, thereby improving production efficiency. On the other hand, it can also reduce the amount of receiving liquid used, which not only saves costs but is also safe and environmentally friendly.

[0059] It should also be noted that, compared with the traditional nanofiltration membrane treatment system, the nanofiltration membrane treatment system uses high pressure operation, and because more acid is added, that is, the ratio of nickel salt to acid is 1: (4~5), and most of the added acid is a strong acid, such as sulfuric acid or nitric acid, which is very corrosive, so that the added sulfuric acid or nitric acid is easy to corrode the metal pipe, resulting in the metal pipe being unable to maintain a good high pressure state for the nanofiltration membrane treatment system under long-term use, resulting in a decrease in the recovery rate of nickel and acid, and there is also a high safety risk during use. In addition, in practical applications, the separation rate of the acid in the nickel-containing precipitate solution of the nanofiltration membrane treatment system is low, with a maximum of only 85%. This increases the difficulty of subsequent evaporation and concentration of the nickel salt concentrate, that is, the concentration time becomes longer, thereby increasing production energy consumption, and then increasing production costs. Therefore, due to the harsh conditions of the nanofiltration membrane treatment system and its inability to adapt to the separation of the nickel-containing precipitate solution with high acid concentration, the industrial application rate of the nanofiltration membrane treatment system is extremely low, and it cannot be widely promoted.

[0060] It should also be noted that, compared with the traditional chemical reaction method, it is necessary to add three additional chemicals, nickel beans / nickel powder, sulfuric acid, and hydrogen peroxide, to increase the concentration of nickel sulfate in the feed solution. This not only results in a higher production cost of nickel sulfate, but also sulfuric acid and hydrogen peroxide have strong oxidizing properties, which are particularly prone to cause safety accidents if not properly operated. In addition, with the continuous development of new energy, the demand for nickel salts has become more tense, which in turn leads to a shortage of nickel beans / nickel powder. In order to ensure that the market's nickel salt needs can be better met and to avoid the shortage of nickel beans / nickel powder, a new nickel leaching scheme needs to be developed. In addition, the traditional chemical reaction method has poor acid recycling, that is, it produces more wastewater, which is not conducive to environmental protection.

[0061] Therefore, the applicant has found through research that when a diffusion dialysis membrane system is used to treat the nickel-containing precipitated liquid, there is no need to add additional chemicals such as nickel beans / nickel powder, which effectively avoids the phenomenon that the demand for nickel salts becomes tight and causes a shortage of nickel beans / nickel powder. Moreover, the use conditions are not so harsh, that is, there is no need to operate under high pressure conditions, so that the diffusion dialysis membrane system can better adapt to the separation of nickel-containing precipitated liquid with high acid concentration. At the same time, it is used in conjunction with the electrodialysis membrane treatment equipment to concentrate the dilute acid solution, which not only improves the safety factor of the membrane method for treating nickel salts and acids in hydrometallurgy, but also the acid separation rate, nickel ion interception rate and acid recovery rate are as high as 95%, thereby improving the overall profit efficiency. In addition, the entire process does not generate wastewater, which is more conducive to environmental protection and energy saving.

[0062] In some other embodiments, since the nickel salt concentrate obtained by the diffusion dialysis membrane system also contains a small amount of acid, in order to improve the recovery rate of the acid, in some other embodiments, when the nickel salt concentrate is evaporated and concentrated, the concentrated mother liquor produced by the concentration is subjected to nickel carbonate precipitation and washing treatment to obtain distilled water, and the distilled water produced is reused in the receiving liquid of the diffusion dialysis membrane system, which improves the recovery of the acid on the one hand, and achieves that the whole process does not generate wastewater on the other hand, which is more conducive to environmental protection. Further, the concentration of the distilled water evaporated after the nickel carbonate precipitation and washing process is 50mg / L~200mg / L, so as to ensure that the concentration of the receiving liquid returned to the diffusion dialysis membrane system as a whole can be kept consistent, so as to ensure that the H + It can improve the separation speed of nickel salt concentrate and dilute acid solution.

[0063] In order to ensure that the diffusion dialysis membrane system has a high diffusion rate, in some other embodiments, the diffusion dialysis membrane system includes a diffusion dialysis chamber and multiple pairs of ion exchange anion membranes, and each of the ion exchange anion membranes is evenly spaced in the diffusion dialysis chamber to divide the diffusion dialysis chamber into multiple dialysis channels to achieve diffusion dialysis of the nickel-containing precipitated liquid.

[0064] Furthermore, in a preferred embodiment, the number of the ion exchange anion membranes is 9.

[0065] It can be understood that by setting the number of ion exchange anion membranes to 9, it can better adapt to the application of adding fresh water and distilled water to circulate back to the diffusion dialysis membrane system. It should be pointed out that since the fresh water and distilled water added in this application contain relatively low weak acidity, in order to ensure a higher concentration of H + The invention has a faster diffusion speed and a higher acid separation rate. The number of ion exchange membranes is controlled to 9, which is 10 compared with the traditional ion exchange membranes. The dialysis channel is wider, which is more conducive to the addition of fresh water and distilled water. + Migration is ensured to ensure that the nickel-containing precipitated liquid flowing into the unit can undergo diffusion dialysis in the 9 ion exchange membranes more quickly, so as to quickly separate the nickel salt from the acid and shorten the diffusion dialysis time.

[0066] Furthermore, in some other embodiments, the spacing between each of the dialysis channels is 0.8 mm to 1.5 mm.

[0067] It should be noted that since fresh water and distilled water contain relatively low acidity and are used as the receiving liquid in the diffusion dialysis membrane system, the H +As the concentration increases, if the dialysis channel is narrow, that is, the adjacent ion exchange membranes are closely spaced, the concentration difference between the adjacent ion exchange membranes will be small, and it will be impossible to ensure that the nickel-containing precipitated liquid can be separated better and faster. Therefore, the present application reduces the number of ion exchange membranes to increase the width of the dialysis channel, that is, the spacing between the dialysis channels is 0.8mm~1.5mm, thereby increasing the concentration difference between adjacent ion exchange membranes to ensure that the nickel-containing precipitated liquid can diffuse more quickly and reliably in the diffusion dialysis membrane system.

[0068] In some other embodiments, the ion exchange anion membrane is an acid-resistant aromatic polyether composite diffusion membrane.

[0069] It can be understood that since the acid-resistant aromatic polyether composite diffusion membrane has a good three-dimensional structure, mechanical strength and acid resistance, the acid-resistant aromatic polyether composite diffusion membrane can better adapt to the high H + The diffusion of the concentrated nickel-containing precipitate prolongs the service life of the acid-resistant aromatic polyether composite diffusion membrane.

[0070] It should be noted that, since the acid-resistant aromatic polyether composite diffusion membrane has a good three-dimensional structure, when the nickel-containing precipitate enters the acid-resistant aromatic polyether composite diffusion membrane, it can form a three-dimensional structure with a good expansion network. If the spacing between the dialysis channels is small, the spacing between the dialysis channels will be further reduced, resulting in a small concentration difference between adjacent ion exchange anion membranes, which is not conducive to the high H + The concentration of nickel-containing precipitate is rapidly diffused in the diffusion dialysis membrane system. Therefore, the spacing of the dialysis channels of the present application is 0.8 mm to 1.5 mm, which increases the concentration difference between adjacent ion exchange membranes and is beneficial to the high H + The high concentration of nickel-containing precipitated liquid diffuses rapidly in the diffusion dialysis membrane system to quickly separate nickel salt from acid, shortening the diffusion dialysis time. On the other hand, it can reserve space for the expansion of the acid-resistant aromatic polyether composite diffusion membrane, so that the nickel-containing precipitated liquid enters the acid-resistant aromatic polyether composite diffusion membrane to form a three-dimensional network structure with good expansion. The adjacent ion exchange anion membranes can still maintain a relatively good concentration difference, so as to better ensure the high H + The concentrated nickel-containing precipitated liquid diffuses rapidly in the diffusion dialysis membrane system to quickly separate the nickel salt from the acid, thus shortening the diffusion dialysis time.

[0071] It should also be noted that, since the flow ratio of the nickel-containing precipitated liquid to the receiving liquid is 1: (0.85-0.95), compared with the conventional flow ratio of the nickel-containing precipitated liquid to the receiving liquid of 1: 1, the initial water pressure flowing into the diffusion dialysis membrane system is relatively slow, so that the impact force on the acid-resistant aromatic polyether composite diffusion membrane adjacent to the inlet is small, and the spacing of the dialysis channels adjacent to the inlet is not easy to change under long-term use, thereby ensuring that the initial section of the nickel-containing precipitated liquid flowing into the diffusion dialysis membrane system still has a good diffusion speed, thereby ensuring that the nickel-containing precipitated liquid has a relatively high H + The concentrated nickel-containing precipitated liquid diffuses rapidly in the diffusion dialysis membrane system to quickly separate the nickel salt from the acid, thus shortening the diffusion dialysis time.

[0072] Furthermore, the pore size of the acid-resistant aromatic polyether composite diffusion membrane is 1 nm to 5 nm, so that the acid-resistant aromatic polyether composite diffusion membrane with a pore size of 1 nm to 5 nm can better adapt to the high H + Rapid diffusion of concentrated nickel-containing precipitate in a diffusion dialysis membrane system.

[0073] The present application also provides a positive electrode material for a battery, comprising the nickel salt product prepared by treating a nickel salt and an acid by a hydrometallurgical membrane method as described in at least any of the above embodiments. The nickel salt product prepared by treating a nickel salt and an acid by a hydrometallurgical membrane method as described in any of the above embodiments can be directly used in preparing a ternary precursor material to provide raw materials for a positive electrode material for a battery.

[0074] Compared with the prior art, the present invention has at least the following advantages:

[0075] The above-mentioned hydrometallurgical membrane method for treating nickel salts and acids, since this method uses a diffusion dialysis membrane system to treat the nickel-containing precipitate liquid, belongs to physical separation, and can obtain nickel salts with better structure and higher purity at room temperature, that is, the acid separation rate reaches 95%, and the nickel ion interception rate reaches 98%, so that the obtained nickel salt can be directly used in the preparation of nickel-hydrogen, nickel-cadmium batteries and nickel-cobalt hydroxide. Compared with the traditional treatment process, since the diffusion dialysis membrane system does not need to add chemicals, it is not only simple and safe to operate, but also low in cost. At the same time, the dilute acid solution is concentrated in conjunction with the electrodialysis membrane treatment equipment to ensure that the H in the diffusion dialysis membrane + It can be maintained within a certain concentration to ensure that the diffusion dialysis membrane system can continuously circulate and operate, and the entire process does not generate wastewater, which is more conducive to environmental protection and energy saving.

[0076] Some specific examples are given below, and if % is mentioned, it means percentage by weight. It should be noted that the following examples do not exhaust all possible situations, and the materials used in the following examples can be obtained from commercial sources unless otherwise specified.

[0077] (1) Crushing and screening: obtaining nickel-containing ore; crushing and screening the nickel-containing ore to obtain nickel-containing ore particles; crushing the nickel-containing ore using a coarse crushing device, crushing the crushed nickel-containing ore to 0.84 mm, and sieving the crushed nickel-containing ore through 20 meshes to obtain nickel-containing ore particles with a smaller particle size;

[0078] (2) Leaching: 10 kg of nickel-containing ore particles are put into a reaction tank, sulfuric acid is added at a ratio of 1:4.6, and the pH is controlled to be 0.8, and a nickel-containing mixed solution is obtained by reaction. The nickel-containing mixed solution is subjected to a filter press operation to obtain nickel-containing ore particles and a nickel-containing leaching solution. The nickel-containing ore particles are returned to the reaction tank for further leaching. When the sulfuric acid concentration of the nickel-containing leaching solution reaches 100 g / L, the nickel-containing leaching solution enters the next process;

[0079] (3) Impurity removal and filtration: nickel carbonate is added to the nickel-containing leaching solution to adjust the pH to 2.0, and an impurity remover is added to precipitate impurities, wherein the impurity remover includes 1L (Fe: 1g / L) mixed solution, 8mL7.8% H2O2, and 2.5mL85% H3PO4 phosphoric acid. The nickel-containing leaching solution after impurity removal is aged, and the aged nickel-containing leaching solution is pumped into a filter press for solid-liquid separation. The filtrate obtained is the nickel-containing precipitated solution, the main components of which are a mixed solution of nickel sulfate and sulfuric acid. When the concentration of sulfuric acid in the nickel-containing precipitated solution reaches 100g / L, it enters the next process;

[0080] (4) Diffusion dialysis membrane system: The nickel-containing precipitated liquid is treated by a diffusion dialysis membrane system to obtain a nickel sulfate concentrate and a dilute sulfuric acid solution. The membrane inlet requirements of the diffusion dialysis membrane system are: suspended solids 0.9 mg / L; H + The concentration is 6 mol / L, the total concentration of nickel salt: the total concentration of acid is 1:10; COD is 100 mg / L; the operating parameters of the diffusion dialysis membrane system are: operating temperature: 35°C, and the dialysis coefficient is 15*10 -7 m / s, acid salt separation factor 40, the flow ratio of the nickel-containing precipitated liquid to the receiving liquid is 1:0.95;

[0081] (5) Evaporation and concentration: The nickel sulfate concentrate is pumped into a nickel sulfate MVR evaporation and concentration device for evaporation and concentration to obtain a nickel sulfate product and a small amount of concentrated mother liquor, and the concentrated mother liquor is subjected to a nickel carbonate precipitation and washing process to obtain a nickel sulfate product containing H +Distilled water with a concentration of 200 mg / L is used back into the diffusion dialysis membrane system as a receiving liquid;

[0082] (6) Concentrated acid in the electrodialysis membrane system: The dilute sulfuric acid solution is pumped into the homogeneous electrodialysis membrane treatment equipment for concentration to obtain a sulfuric acid product with a concentration of 180 g / L and a sulfuric acid product containing H + Fresh water with a concentration of 200 mg / L is recycled into the diffusion dialysis membrane system as a receiving liquid, and the sulfuric acid product is compounded with concentrated sulfuric acid to obtain a sulfuric acid solution used in the leaching step.

[0083] (1) Crushing and screening: obtaining nickel-containing ore; crushing and screening the nickel-containing ore to obtain nickel-containing ore particles; crushing the nickel-containing ore using a coarse crushing device, crushing the crushed nickel-containing ore to 0.75 mm, and sieving the crushed nickel-containing ore through 10 meshes to obtain nickel-containing ore particles with a smaller particle size;

[0084] (2) Leaching: 10 kg of nickel-containing ore particles are put into a reaction tank, sulfuric acid is added at a ratio of nickel salt to sulfuric acid of 1:4.5, and the pH is controlled to be 0.9, and a nickel-containing mixed solution is obtained by reaction, and a filter press operation is performed on the nickel-containing mixed solution to obtain nickel-containing ore particles and a nickel-containing leaching solution. The nickel-containing ore particles are returned to the reaction tank for further leaching. When the sulfuric acid concentration of the nickel-containing leaching solution is 70 g / L, the nickel-containing leaching solution enters the next process;

[0085] (3) Impurity removal and filtration: nickel carbonate is added to the nickel-containing leaching solution to adjust the pH to 2.0, and an impurity remover is added to precipitate impurities, wherein the impurity remover includes 1L (Fe: 1g / L) mixed solution, 8mL7.8% H2O2, and 2.5mL85% H3PO4 phosphoric acid. The nickel-containing leaching solution after impurity removal is aged, and the aged nickel-containing leaching solution is pumped into a filter press for solid-liquid separation. The filtrate obtained is the nickel-containing precipitated solution, the main components of which are a mixed solution of nickel sulfate and sulfuric acid. When the concentration of sulfuric acid in the nickel-containing precipitated solution reaches 70g / L, it enters the next process;

[0086] (4) Diffusion dialysis membrane system: The nickel-containing precipitated liquid is treated by a diffusion dialysis membrane system to obtain a nickel sulfate concentrate and a dilute sulfuric acid solution. The membrane inlet requirements of the diffusion dialysis membrane system are: suspended solids 0.8 mg / L; H + The concentration is 1mol / L, the total concentration of nickel salt: the total concentration of acid is 0.6:10; COD is 150mg / L; the operating parameters of the diffusion dialysis membrane system are: operating temperature: 15℃, and the dialysis coefficient is 20*10 -7 m / s, acid salt separation factor 40, the flow ratio of the nickel-containing precipitated liquid to the receiving liquid is 1:0.85;

[0087] (5) Evaporation and concentration: The nickel sulfate concentrate is pumped into a nickel sulfate MVR evaporation and concentration device for evaporation and concentration to obtain a nickel sulfate product and a small amount of concentrated mother liquor, and the concentrated mother liquor is subjected to a nickel carbonate precipitation and washing process to obtain a nickel sulfate product containing H + Distilled water with a concentration of 50 mg / L is used back into the diffusion dialysis membrane system as a receiving liquid;

[0088] (6) Concentrated acid in the electrodialysis membrane system: The dilute sulfuric acid solution is pumped into the homogeneous electrodialysis membrane treatment equipment for concentration to obtain a sulfuric acid product with a concentration of 120 g / L and a H + Fresh water with a concentration of 50 mg / L is reused in the diffusion dialysis membrane system as a receiving liquid, and the sulfuric acid product is compounded with concentrated sulfuric acid to obtain a sulfuric acid solution used in the leaching step.

[0089] Comparative Example 1

[0090] The difference from Example 1 is that step (4) is different. In step (4) of Comparative Example 1, a nanofiltration membrane system is used, that is, the nickel-containing precipitated liquid is transported to the nanofiltration membrane treatment system to obtain a concentrated nickel sulfate solution and a sulfuric acid solution, respectively; the rest remains unchanged.

[0091] Comparative Example 2

[0092] The difference from Example 1 is that step (4) is different and step (6) is missing. In Comparative Example 2, step (4) is a chemical reaction, that is, nickel beans / nickel powder, sulfuric acid and hydrogen peroxide are added to the nickel-containing precipitate liquid for reaction, and then step (5) is entered without step (6), and the rest remains unchanged.

[0093] The various costs, safety risks, acid separation rate, and nickel ion interception rate of the above Example 1 and Comparative Examples 1-2 were analyzed and compared to obtain the following Table 1:

[0094] project Example 1 Comparative Example 1 Comparative Example 2 Output products Nickel sulfate hexahydrate + sulfuric acid Nickel sulfate hexahydrate + sulfuric acid Nickel sulfate hexahydrate Investment and construction costs 215 yuan / m³ 180 yuan / m³ 75 yuan / m³ Operating costs 134 yuan / m³ 106 yuan / m³ 3075 yuan / m³ Product Benefits 4507 yuan / m³ 4507 yuan / m³ 7200 yuan / m³ Overall process benefit comparison 4158 yuan / m³ 4221 yuan / m³ 4050 yuan / m³ System operation security risks Low high Higher Acid separation rate 95% 85% 98% Nickel ion interception rate 98% 90% / Acid recovery 95% 85% /

[0095] It can be seen from Example 1 and Comparative Examples 1-2 that the diffusion dialysis membrane system and electrodialysis membrane treatment equipment used in Example 1 to treat the nickel-containing post-precipitation liquid not only has good economic benefits, but is also safe and environmentally friendly, and the acid separation rate, nickel ion interception rate and acid recovery rate are as high as 95%, so that the various indicators of Example 1 are significantly better than those of Comparative Examples 1-2.

[0096] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as a restriction on the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for treating nickel salts and acids by membrane method in hydrometallurgy, characterized in that: The steps include: Obtaining nickel-containing ore; Crushing and screening the nickel-containing ore to obtain nickel-containing ore particles; The nickel-containing ore particles are leached with an acid solution to obtain a nickel-containing mixed solution; wherein the ratio of the nickel salt to the acid is 1:(4-5); The nickel-containing mixed solution is filtered to remove impurities to obtain a nickel-containing precipitated solution; and the nickel-containing precipitated solution is pumped into a diffusion dialysis membrane treatment system only when the acid concentration in the nickel-containing precipitated solution is ≥70 g / L; The nickel-containing precipitated liquid is treated by a diffusion dialysis membrane system to obtain a nickel salt concentrate and a dilute acid solution; wherein, when the nickel-containing precipitated liquid is treated by a diffusion dialysis membrane system, the membrane entry requirements are: suspended solids <1.0 mg / L, H + Concentration ≤6mol / L, total nickel salt concentration: total acid concentration ≤1:10, COD<200mg / L, operating temperature: 15℃~45℃; dialysis coefficient 10*10 -7 m / s~20*10 -7 m / s, acid salt separation factor 40; the diffusion dialysis membrane system comprises a feed liquid and a receiving liquid, the feed liquid and the receiving liquid flow in countercurrent, the feed liquid is a nickel-containing precipitated liquid, the concentration of the receiving liquid is 50 mg / L~200 mg / L; and the flow ratio of the nickel-containing precipitated liquid to the receiving liquid is 1:(0.85~0.95); The diffusion dialysis membrane system comprises a diffusion dialysis chamber and a plurality of pairs of ion exchange anion membranes, wherein the ion exchange anion membranes are evenly spaced in the diffusion dialysis chamber to divide the diffusion dialysis chamber into a plurality of dialysis channels, and the spacing between each of the dialysis channels is 0.8 mm to 1.5 mm; the nickel salt concentrate is evaporated and concentrated to obtain a nickel salt product; The dilute acid solution is concentrated by electrodialysis membrane treatment equipment to obtain an acid product.

2. The method for treating nickel salt and acid by membrane method in hydrometallurgy according to claim 1, characterized in that: When the nickel-containing precipitated liquid is treated by a diffusion dialysis membrane system, the pH of the nickel-containing precipitated liquid is 1.5-3.

0.

3. The method for treating nickel salt and acid by membrane method in hydrometallurgy according to claim 1, characterized in that: The electrodialysis membrane treatment equipment has an ion exchange capacity of 0.8 mol / Kg to 1.5 mol / Kg, a migration number > 0.97, and a membrane resistance of 2.8 Ωm / cm 2 ~3.5Ωm / cm 2 Concentrated under the conditions.

4. The method for treating nickel salt and acid by membrane method in hydrometallurgy according to claim 1, characterized in that: After the step of concentrating the dilute acid solution by electrodialysis membrane treatment equipment to obtain an acid product, the following steps are also included: The acid solution is obtained by compounding the acid product with a concentrated acid.

5. The method for treating nickel salt and acid by membrane method in hydrometallurgy according to claim 1, characterized in that: The concentration of the acid product is ≥120 g / L.

6. The method for treating nickel salt and acid by membrane method in hydrometallurgy according to claim 1, characterized in that: The step of evaporating and concentrating the nickel salt concentrate comprises the following specific steps: The nickel salt concentrate is pumped into the nickel salt MVR evaporation concentration equipment for evaporation concentration and impurity removal.

7. A positive electrode material for a battery, characterized in that: The nickel salt product is prepared by the method for treating nickel salt and acid by membrane method in hydrometallurgy as described in at least any one of claims 1 to 6.