A copper-based catalyst for catalytic hydrogenation of dimethyl oxalate and its preparation method and application
A copper-silver nanosphere catalyst supported by hydrothermal synthesis was prepared, which allowed Cu+ active sites to be gradually released during hydrogen pre-reduction and reaction. This solved the problem of easy aggregation of copper-based catalysts, resulting in a highly active and stable copper-based catalyst with extended service life.
Patent Information
- Application Number
- CN202211606617.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-13
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-13
AI Technical Summary
Existing copper-based catalysts have a short lifespan in the hydrogenation of oxalate esters, mainly because Cu0 active sites tend to agglomerate during the reduction reaction, leading to an imbalance in the Cu+/Cu0 ratio and affecting catalyst performance and stability.
A hydrothermal synthesis method was used to prepare copper-silver nanosphere catalysts, which allowed Cu+ active sites to be gradually released during hydrogen pre-reduction and reaction, maintaining a high Cu+/Cu0 ratio, inhibiting the reduction of Cu+ to Cu0, and extending the catalyst lifetime.
This study achieved high activity and high stability of the catalyst in the catalytic hydrogenation reaction of lower fatty acid esters, thus extending the catalyst's lifespan.
Smart Images

Figure BDA0003996059120000061 
Figure HHA0000007023030000011 
Figure HHA0000007023030000021
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing a copper-based catalyst for catalytic hydrogenation of low-level fatty acid esters, which can gradually release active sites during hydrogen pre-reduction and reaction. Specifically, it relates to a method for preparing a copper-based catalyst for catalytic hydrogenation of dimethyl oxalate, which can gradually release active sites during hydrogen pre-reduction and reaction. Background Art
[0002] Coal-to-ethylene glycol technology is a process technology that uses coal to produce synthesis gas; then uses CO and H2 in the synthesis gas as raw materials to synthesize oxalate, which is further hydrogenated to produce ethylene glycol. The catalyst used for the hydrogenation of dimethyl oxalate to produce ethylene glycol is mainly a copper-based catalyst, which has good performance in industry, but also has problems such as short service life. Therefore, how to improve the service life of oxalate hydrogenation catalyst is a key technical issue in coal-to-ethylene glycol technology and also a technical difficulty in this field. The Hüttig temperature of Cu (~134°C) is much lower than the reaction temperature of dimethyl oxalate hydrogenation (180~200°C), which can easily cause sintering of the catalyst, which is also the main reason for the deactivation of copper-based catalysts. It is generally believed that Cu 0 The active site plays a role in activating and dissociating H2, Cu + The active sites promote the activation and adsorption of methoxy or acyl groups in ester molecules, and the two synergistically catalyze the hydrogenation reaction of esters. Ma Xinbin et al. (ACS Catalysis, 2015, 5: 6200–6208) believe that when Cu on the catalyst surface 0 When species are relatively abundant, Cu + Ma Xiangang et al. (RSC advances, 2015, 5: 37581-37584) found that esters (methyl acetate, ethyl acetate, dimethyl oxalate) can convert Cu in Cu / SiO2 catalyst into 0 Oxidation to Cu + , Cu + It will be reduced to Cu by H2 in the reaction atmosphere. 0 , so Cu + and Cu 0 will convert to each other, achieving a dynamic redox cycle. 0 The Huttig temperature is low, and it is easy to agglomerate and grow into large particles during the reduction reaction, resulting in the loss of some active sites and destroying the Cu + / Cu 0 The dynamic redox cycle of Cu + / Cu 0 The ratio is unbalanced, which reduces the performance of the catalyst or even makes it inactive.
[0003] In recent years, people have adopted a variety of measures to improve the service life of copper-based catalysts. One of the important measures is to introduce a second metal additive into the copper-based catalyst to form a Cu-M bimetallic alloy phase with the copper species to regulate the charge state and distribution of the active species. For example, trace metal elements and copper form bimetallic species, which not only helps to obtain a suitable Cu + / Cu 0 ratio, and can also promote its adsorption and activation of C=O / C–O bonds in ester molecules, and can effectively prevent the aggregation of metal copper nanoparticles (Cu NPs), significantly improving the ester hydrogenation performance of the catalyst. Chinese patent CN114054024A reported a dimethyl oxalate hydrogenation catalyst and its preparation method and application, the main active component is copper, and the auxiliary active component is a metal selected from Ni, In, Mo, W, Fe, Zn and / or its oxide. In the catalytic hydrogenation reaction of dimethyl oxalate, the conversion rate of dimethyl oxalate is greater than 99.8%, and the selectivity of ethylene glycol reaches 99.0%. Chinese patent CN110142048A reports a silver-copper catalyst for hydrogenating dimethyl oxalate to synthesize methyl glycolate, and its preparation method and use method, wherein the catalyst with active component Ag-Cu and carrier MgO-Al2O3 is used in the catalytic hydrogenation reaction of hydrogenating dimethyl oxalate to synthesize methyl glycolate, when the reaction temperature is 220°C, the hydrogen pressure is 3MPa, and the hydrogen-ester ratio is 250, the conversion of dimethyl oxalate can reach 86.6%, and the selectivity of methyl glycolate can reach 84.4%. Chinese patent CN105457631A reports a silver-silicon catalyst, which can achieve a conversion of dimethyl oxalate of 95% and a selectivity of methyl glycolate of 91% in the hydrogenation reaction of dimethyl oxalate. Chinese patent CN107303488B reports a silver silicon catalyst. When the reaction temperature is 210°C, the hydrogen pressure is 3.5 MPa, and the hydrogen-ester ratio is 150, the conversion of dimethyl oxalate can reach 100%, and the selectivity of ethylene glycol can reach 95.5%.
[0004] Many research reports have shown that the introduction of new metal elements as additives can potentially change the Cu 0 and Cu + Equal number of active sites, Cu + / Cu 0 The present invention introduces a method for gradually releasing monovalent copper (Cu + ) active site of the copper-based catalyst preparation method, namely Cu + The active sites are gradually released during the hydrogen pre-reduction and reaction process. This invention not only enables the copper-based catalyst to gradually release monovalent copper (Cu) in the catalytic hydrogenation reaction of low-level fatty acid esters, but also can effectively reduce the active sites of the catalyst. +) active sites, and can also maintain a high Cu + / Cu 0 ratio, effectively inhibiting Cu + The species is reduced to Cu during the reaction. 0 species, thereby maintaining high activity and stability of the copper-based catalyst. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a copper-based silicon catalyst for catalytic hydrogenation of low-level fatty acid esters, which can gradually release active sites during hydrogen pre-reduction and reaction. + The active sites ensure that the catalyst can be activated quickly and can continuously release Cu during the reaction. + Active sites, which not only enable the catalyst to exhibit higher catalytic hydrogenation performance, but also increase the service life of the catalyst.
[0006] The technical scheme of the present invention is: firstly, tetraethyl orthosilicate is used as a silicon source, and nano silicon spheres are prepared by hydrothermal synthesis, and then the nano silicon spheres are mixed with soluble copper salt and silver salt to form a mixed solution, and then hydrothermal synthesis is performed to prepare a nano silicon sphere catalyst loaded with copper and silver. The catalyst has high activity and high stability at a relatively low reaction temperature.
[0007] The preparation steps of the copper-based catalyst of the present invention are:
[0008] A. Add a certain volume of tetraethyl orthosilicate and anhydrous ethanol to a certain volume of deionized water, then add a certain volume of ammonia water, and continue stirring at 40°C for 3 hours to obtain a suspension containing nano-silicon spheres. The suspension is centrifuged and washed several times with an ethanol aqueous solution with a volume ratio of ethanol to water of 1:1 to obtain nano-silicon sphere powder. The volume ratio of tetraethyl orthosilicate to anhydrous ethanol is 1:4 to 1:10, the volume ratio of tetraethyl orthosilicate to deionized water is 1:2 to 1:6, the mass percentage concentration of ammonia water is 25%, and the volume ratio of tetraethyl orthosilicate to ammonia water is 1:0.5 to 1:1.5.
[0009] B. Dissolve the nano-silicon spheres obtained in step A in a certain volume of deionized water to form a turbid liquid containing nano-silicon spheres.
[0010] C. Dissolve a certain mass of soluble copper salt and silver salt in a certain volume of deionized water to form a copper ion and silver ion solution of a certain concentration, then add a certain volume of ammonia water, stir, and then add the nano-silicon ball turbid solution described in step B, stir until fully mixed, and form a uniform mixed solution. The soluble copper salt is one of copper nitrate or copper oxalate, and the soluble silver salt is silver nitrate, wherein the copper ion concentration is 0.05mol / L to 0.4mol / L, the silver ion concentration is 0.005mol / L to 0.1mol / L, the molar ratio of silver element to copper element is 0.02 to 0.4, and the molar ratio of silver element to silicon element is 0.02 to 0.3.
[0011] D. Transfer the mixed solution of step C to a hydrothermal kettle, place it in an oven and perform hydrothermal synthesis at a certain temperature for a certain time, and after the hydrothermal kettle is naturally cooled, obtain a solid-liquid mixture and centrifuge it, and wash it three times with deionized water to obtain a filter cake. The temperature of the hydrothermal synthesis is 120-200° C., and the hydrothermal synthesis time is 12-48 hours.
[0012] E. The filter cake obtained in step D is placed in an oven, dried at a certain temperature for several hours, and then transferred to a muffle furnace, and roasted at a certain temperature for a certain time to obtain a solid powder. Finally, the solid powder is pressed into tablets and sieved to obtain particles with a particle diameter of 0.25 to 0.40 mm, the drying temperature is 60 to 100° C., the time is 6 to 24 hours, and the roasting temperature is 300 to 600° C., and the time is 3 to 12 hours.
[0013] The reduction and reaction method of copper-based catalyst in the hydrogenation of dimethyl oxalate to synthesize ethylene glycol is as follows: the catalyst sample is loaded into a tubular fixed bed reactor, and in a nitrogen atmosphere with a flow rate of 50 ml / min, the temperature is increased from room temperature to 150°C at a rate of 2°C / min, and then switched to hydrogen, and the temperature is continued to be increased to 300°C and maintained for 3 to 10 hours, and then the system temperature is lowered to the reaction temperature, and a prepared methanol solution containing 0.2 g / ml dimethyl oxalate is introduced into a vaporization chamber and mixed with hydrogen, the hydrogen / dimethyl oxalate molar ratio is 20 to 100, and the reaction is carried out at a reaction temperature of 170 to 200°C for 24 to 7 hours, and the liquid hourly space velocity of dimethyl oxalate is 0.2 to 2.0 g / g·h.
[0014] The content of monovalent copper on the surface of the copper-based catalyst after the hydrogenation reaction of dimethyl oxalate is significantly increased compared with the content of monovalent copper on the surface of the copper-based catalyst before the reaction. The difference between the content of monovalent copper on the surface of the catalyst after the reaction and the content of monovalent copper on the surface of the catalyst before the reaction is 15% to 40%.
[0015] The beneficial effects of the present invention are as follows: the present invention adopts a relatively simple method to make monovalent copper (Cu +) is gradually released during the pre-reduction and reaction of dimethyl oxalate catalytic hydrogenation, slowing down the release of monovalent copper (Cu + ) The rate at which the active sites are reduced and agglomerated keeps a high Cu + / Cu 0 ratio, thereby maintaining high activity and stability of the copper-based catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The X-ray diffraction spectra of comparative example 1 and example 1 after reduction (before reaction) and reaction for 72 hours, curve A represents example 1 after reduction (before reaction), curve B represents example 1 after reduction, curve C represents comparative example 1 after reduction (before reaction), and curve D represents comparative example 1 after reaction.
[0017] Figure 2 The X-ray photoelectric energy spectra of comparative example 1 and example 1 after reduction (before reaction) and after reaction for 72 hours, curve A represents example 1 after reduction (before reaction), curve B represents example 1 after reduction, curve C represents comparative example 1 after reduction (before reaction), and curve D represents comparative example 1 after reaction.
[0018] Figure 3 The activity evaluation results of Comparative Example 1 and Example 1 at 180°C for 500 hours are shown. Curves A and C represent the conversion rates of dimethyl oxalate in Example 1 and Comparative Example 1, respectively. Curves B and D represent the selectivity of ethylene glycol in Example 1 and Comparative Example 1, respectively. DETAILED DESCRIPTION
[0019] Embodiment 1:
[0020] Preparation method:
[0021] A. Add 8 mL of tetraethyl orthosilicate and 45 mL of anhydrous ethanol to 25 mL of deionized water, then add 9 mL of 25 wt% ammonia water, and continue stirring at 40°C for 3 h to obtain a suspension containing nano-silicon spheres. The suspension is centrifuged and washed several times with an ethanol-water solution having a volume ratio of ethanol to water of 1:1 to obtain nano-silicon sphere powder.
[0022] B. Add the nano-silicon sphere powder obtained in step A into 35 mL of deionized water to form a turbid solution containing nano-silicon spheres.
[0023] C. Dissolve 0.42 g of silver nitrate and 4.5 g of copper nitrate in 100 g of deionized water, then add 16 mL of 25 wt% ammonia water, stir for 15 minutes, then add the turbid solution containing nano-silicon spheres described in step B, stir until fully mixed to form a uniform mixed solution.
[0024] D. The mixed solution in C was transferred to a 200 mL hydrothermal kettle and placed in an oven to heat at 160° C. for 20 h. After the hydrothermal kettle was cooled naturally, a solid-liquid mixture was obtained and centrifuged and filtered, and washed three times with deionized water to obtain a filter cake.
[0025] E. The filter cake obtained in D is placed in an oven and dried at 70°C for 24 hours, then transferred to a muffle furnace and calcined at 400°C for 5 hours to obtain a solid powder, and finally the obtained solid powder is pressed into tablets and sieved into particles with a diameter of 0.25 to 0.40 mm.
[0026] Performance evaluation:
[0027] The copper-based catalyst precursor particles with a diameter of 0.25 to 0.40 mm were loaded into a tubular fixed bed reactor. In a nitrogen atmosphere with a pressure of 1.0 MPa and a flow rate of 50 ml / min, the temperature was raised from room temperature to 150 ° C at a rate of 2 ° C / min, and then switched to hydrogen. The temperature was further raised to 300 ° C and maintained for 5 hours, then the temperature was lowered to the reaction temperature of 180 ° C, and the reaction hydrogen pressure was raised to 2.0 MPa for performance evaluation. At the same time, the prepared 0.2 g / ml dimethyl oxalate methanol solution was introduced into the vaporization chamber and mixed with hydrogen to carry out oxalate hydrogenation reaction, wherein H2 / DMO=50 (mol / mol), and the liquid hourly space velocity of dimethyl oxalate was 1.0 g (DMO) / gcat·h. The results of the selective hydrogenation of dimethyl oxalate to synthesize ethylene glycol for 72 hours are shown in Table 1. The surface Cu before the reaction (after reduction) and after 72 hours and 500 hours of reaction are shown in Table 1. + The content and its increment results are shown in Tables 2 and 3. The X-ray diffraction spectra and X-ray photoelectric spectrum after reduction (before reaction) and after 72 hours of reaction, as well as the activity evaluation results at 180°C for 500 hours are shown in the appendix of the manual. Figure 1 , 2, 3.
[0028] Embodiment 2:
[0029] In Example 1, the mass of silver nitrate in Step C is changed to 0.13 g, which is the same as this example.
[0030] The performance evaluation conditions were the same as those in Example 1. The results of the selective hydrogenation of dimethyl oxalate to ethylene glycol after 72 hours are shown in Table 1. Surface Cu before reaction (after reduction) and after 72 hours of reaction + The contents and their increment results are shown in Table 2.
[0031] Embodiment 3:
[0032] In Example 1, the mass of silver nitrate in Step C is changed to 1.0 g, that is, this example.
[0033] The performance evaluation conditions were the same as those in Example 1. The results of the selective hydrogenation of dimethyl oxalate to ethylene glycol after 72 hours are shown in Table 1. The surface Cu + The contents and their increment results are shown in Table 2.
[0034] Embodiment 4:
[0035] In Example 1, placing in an oven at 160° C. in step D is changed to placing in an oven at 180° C., that is, this example.
[0036] The performance evaluation conditions were the same as those in Example 1. The results of the selective hydrogenation of dimethyl oxalate to ethylene glycol after 72 hours are shown in Table 1. The surface Cu + The contents and their increment results are shown in Table 2.
[0037] Embodiment 5:
[0038] In Example 1, the heating for 20 hours in step D is changed to placing in an oven for 36 hours, which is the present example.
[0039] The performance evaluation conditions were the same as those in Example 1. The results of the selective hydrogenation of dimethyl oxalate to ethylene glycol after 72 hours are shown in Table 1. The surface Cu + The contents and their increments are shown in Table 2.
[0040] Comparative Example 1
[0041] In Example 1, the mass of silver nitrate in Step C is changed to 0 g, that is, this example.
[0042] The performance evaluation conditions were the same as those in Example 1. The results of the selective hydrogenation of dimethyl oxalate to ethylene glycol after 72 h are shown in Table 1. The surface Cu + The content and its increment results are shown in Tables 2 and 3. The X-ray diffraction spectra and X-ray photoelectric spectrum after reduction (before reaction) and after 72 hours of reaction, as well as the activity evaluation results at 180°C for 500 hours are shown in the appendix of the manual. Figure 1 , 2,3.
[0043] Comparative Example 2
[0044] The steps in Example 1 are changed to: the mixed solution in step C is transferred to a beaker, placed in a water pot at 80° C. to evaporate ammonia until the liquid is neutral, the solid-liquid mixture obtained after the ammonia evaporation is filtered, and washed three times with deionized water to obtain a filter cake, which is this example.
[0045] The performance evaluation conditions were the same as those in Example 1. The results of the selective hydrogenation of dimethyl oxalate to ethylene glycol after 72 hours are shown in Table 1. The surface Cu+ The contents and their increment results are shown in Table 2.
[0046] Table 1 Catalyst activity evaluation results for each case
[0047] Oxalate conversion rate, % Ethylene glycol selectivity, % Example 1 99.98 97.20 Example 2 99.98 90.71 Example 3 99.93 88.50 Example 4 99.98 97.07 Example 5 99.98 96.53 Comparative Example 1 98.85 65.24 Comparative Example 2 96.75 59.19
[0048] Table 2 Surface Cu of each catalyst after reduction (before reaction) and after reaction for 72h + Content and its increment results
[0049] Note: Surface Cu + The content is calculated based on X-ray photoelectron spectroscopy. + Content and surface Cu before and after reaction (after reduction) + The difference in content is the surface Cu + The increase in content can be seen from Table 2. + The content increased by 19-30.7%.
[0050] Table 3 Surface Cu after reaction for 500 h in Example and Comparative Example 1 + Content results
[0051] <![CDATA[Cu content after 500h reaction, %]]> + Content, %]]> Example 1 64.2 Comparative Example 1 56.2
[0052] Note: Surface Cu + The content was calculated based on X-ray photoelectron spectroscopy.
Claims
1. A method for preparing a copper-based catalyst for catalytic hydrogenation of dimethyl oxalate, characterized in that: A. Add tetraethyl orthosilicate and anhydrous ethanol to deionized water, then add ammonia water, and continue stirring at 40 °C for 3 hours to obtain a suspension containing nano-silicon spheres; the suspension is centrifuged and washed several times with an ethanol aqueous solution with a volume ratio of ethanol to water of 1:1 to obtain nano-silicon spheres; wherein the volume ratio of tetraethyl orthosilicate to anhydrous ethanol is 1:4-1:10, the volume ratio of tetraethyl orthosilicate to deionized water is 1:2-1:6, the mass percentage concentration of ammonia water is 25%, and the volume ratio of tetraethyl orthosilicate to ammonia water is 1:0.5-1:1.5; B. dissolving the nano-silicon spheres obtained in step A in deionized water to form a turbid solution containing nano-silicon spheres; the volume ratio of tetraethyl orthosilicate in step A to deionized water in step B is 8:35; C. dissolving soluble copper salt and silver salt in deionized water to form a solution containing copper ions and silver ions, then adding ammonia water, stirring and then adding the nano-silicon ball turbid solution described in step B, wherein the mass percentage concentration of ammonia water is 25%, and the volume ratio of tetraethyl orthosilicate in step A to ammonia water in step C is 1:2; stirring until fully mixed to form a uniform mixed solution; the soluble copper salt is one of copper nitrate or copper oxalate, and the soluble silver salt is silver nitrate, wherein the copper ion concentration is 0.05mol / L-0.4mol / L, the silver ion concentration is 0.005mol / L-0.1mol / L, the molar ratio of silver element to copper element is 0.02-0.4, and the molar ratio of silver element to silicon element is 0.02-0.3; D. Transfer the mixed solution of step C to a hydrothermal reactor for hydrothermal synthesis. After the hydrothermal reactor is naturally cooled, a solid-liquid mixture is obtained and centrifuged and filtered. The filter cake is washed three times with deionized water. The temperature of the hydrothermal synthesis is 120 to 200 ° C, and the hydrothermal synthesis time is 12 to 48 hours. E. The filter cake obtained in step D is placed in an oven for drying, and then transferred to a muffle furnace for calcination to obtain a solid powder; finally, the solid powder is pressed into tablets and sieved to obtain particles with a particle diameter of 0.25 to 0.40 mm, the drying temperature is 60 to 100°C, the time is 6 to 24 hours, and the calcination temperature is 300 to 600°C, and the time is 3 to 12 hours; After the catalyst is used for the hydrogenation reaction of dimethyl oxalate, the content of monovalent copper on the surface of the copper-based catalyst increases significantly. The content of monovalent copper on the surface of the catalyst after the reaction increases by 15% to 40% compared with the content of monovalent copper on the surface of the catalyst before the reaction.
2. The use of the copper-based catalyst prepared by the method of claim 1, characterized in that: The catalyst sample was loaded into a tubular fixed-bed reactor. In a nitrogen atmosphere with a flow rate of 50 mL / min, the temperature was raised from room temperature to 150 °C at a rate of 2 °C / min, then switched to hydrogen. The temperature was continued to rise to 300 °C and maintained for 3 to 10 h. The system temperature was then lowered to the reaction temperature. A prepared methanol solution containing 0.2 g / mL dimethyl oxalate was introduced into the vaporization chamber and mixed with hydrogen in a hydrogen / dimethyl oxalate molar ratio of 20 to 100. The reaction was carried out at a reaction temperature of 170 to 200 °C for 24 to 72 h. The liquid hourly space velocity of dimethyl oxalate was 0.2 to 2.0 g / (g•h).