Glycolide purification method, refined glycolide, and application
Through the liquid separation purification method of isopropanol and glycolide crude product, the problems of low purity, low purity and high process cost in the prior art were solved, and efficient purification of high purity glycolide was achieved. , suitable for the preparation of degradable polymer materials.
Patent Information
- Application Number
- CN202310130074.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-17
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-02-17
AI Technical Summary
The existing glycolide purification methods have problems such as low product yield, low purity, high process cost and insufficient ability to reduce free acid value.
The crude isopropyl alcohol and glycolide are heated until melted, and left to stand to form a delamination. The upper layer material is collected for cooling, crystallization, filtering and drying. The volume of isopropyl alcohol is controlled to be of 4.5 to 7.5 mL. : Within the range of 1 g, the purification of high-purity glycolide is achieved by liquid separation method.
The purification yield and purity of glycolide were improved, the free acid content was reduced to below 0.030 mmol/g, and the purity reached more than 99.9%, which simplified the process flow and reduced production costs.
Smart Images

Figure CN116082291B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of chemical material synthesis, and in particular to a method for purifying glycolide, refining glycolide, and application thereof. Background Art
[0002] Glycolide is an important monomer for synthesizing biodegradable polymer materials. For example, glycolide can be used to synthesize various polymer materials such as polyglycolic acid, poly(lactide-glycolic acid), and polycaprone. The synthesized materials can be widely used in agricultural materials, packaging materials, fracturing materials, medical polymer materials and other fields.
[0003] The preparation process of glycolide is usually to obtain low molecular weight polyglycolic acid through polycondensation reaction of raw materials such as glycolic acid or methyl glycolate, and then obtain glycolide through high temperature cracking of low molecular weight polyglycolic acid. However, the glycolide prepared by this method is only a crude product and needs to be purified before it can be used as a polymerization raw material.
[0004] Common methods for purifying glycolide include solvent crystallization, melt crystallization, distillation, etc. For example, U.S. Patent No. 4835293A proposes that hot nitrogen gas can be used to carry glycolide vapor into isopropanol for purification at high temperature and normal pressure, but the product yield after purification by this method is low. For example, Japanese Patent No. JP2001278877A provides a melt crystallization device, which has a good purification effect on crude glycolide, but the manufacturing difficulty and cost of the device are high. For another example, Japanese Patent No. JP6326373B2 uses distillation to obtain glycolide with a free acid value between 0.2-0.58 mmol / g, but no further refining process is recorded to ensure the purity of the purified glycolide. For another example, Taiwan Patent No. TW201035116A introduces a mixed solvent to azeotrope with glycolide, and uses a total reflux process to obtain glycolide with a purity of more than 99.0%, but the free acid value reduction ability and product yield of this method cannot be guaranteed. Summary of the invention
[0005] Based on this, it is necessary to provide a method for purifying glycolide, refining glycolide, and application thereof, which can improve product yield and purity and reduce free acid value and process cost.
[0006] An embodiment of the present application provides a method for purifying glycolide, comprising the following steps:
[0007] Providing crude glycolide to be purified;
[0008] adding isopropanol to the crude glycolide to form a mixture, and heating the mixture until the crude glycolide is melted;
[0009] Let it stand until stratification occurs, and collect the upper layer material;
[0010] Cooling, crystallizing, filtering and drying the upper layer material;
[0011] The volume of the isopropanol added per 1 g of the crude glycolide is less than 8 mL.
[0012] In one of the embodiments, the volume ratio of the isopropanol to the crude glycolide is (4.5-7.5) mL: 1 g.
[0013] In one embodiment, the heating temperature is 75°C to 85°C.
[0014] In one embodiment, the heating temperature is 83°C to 84°C.
[0015] In one embodiment, the crude glycolide is a crude product obtained by polycondensation and cracking of glycolic acid.
[0016] In one embodiment, the process of cooling, crystallizing, filtering and drying the upper material also includes a step of washing the filtered residue.
[0017] In one embodiment, the detergent used for washing is isopropyl alcohol;
[0018] Optionally, the number of washings is 2 to 4 times.
[0019] An embodiment of the present application also provides a refined glycolide, which is purified by the glycolide purification method described in any of the above embodiments.
[0020] In one embodiment, the free acid content of the refined glycolide is ≤0.030 mmol / g; and the purity of the refined glycolide is ≥99.9%.
[0021] An embodiment of the present application also provides a use of the refined glycolide as described in any of the above embodiments in the preparation of a degradable polymer material.
[0022] The above-mentioned method for purifying glycolide is based on the principle of liquid separation method. After the glycolide crude product is mixed with isopropanol and heated, the mixed materials are allowed to stand and stratify, wherein the upper layer material mainly includes a saturated isopropanol solution of glycolide. The upper layer material is collected and cooled, crystallized, filtered and dried to obtain a refined glycolide with low free acid content and high purity, which meets the application requirements for preparing degradable polymer materials. In addition, the purification yield is high, the purification method is simple, and it is conducive to reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the GC test spectrum of the refined glycolide of Example 1;
[0024] Figure 2The DSC test spectra of the crude glycolide prepared in step 2 of Example 1 and the refined glycolide purified in step 3;
[0025] Figure 3 The purified glycolide of Example 1 1 HNMR test spectrum. DETAILED DESCRIPTION
[0026] For ease of understanding of the application, the application is described more fully below in conjunction with embodiments and accompanying drawings. The application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the application more thorough and comprehensive.
[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0028] In the present application, "further", "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present application.
[0029] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0030] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. For example, therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.
[0031] The weight of the relevant components mentioned in the specification of the examples of this application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the specification of the examples of this application, it is within the scope disclosed in the specification of the examples of this application. Specifically, the weight described in the specification of the examples of this application can be mass units known in the chemical industry such as μg, mg, g, and kg.
[0032] The temperature parameters in the present invention, if not specifically limited, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0033] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0034] An embodiment of the present application provides a method for purifying glycolide, comprising the following steps:
[0035] Providing crude glycolide to be purified;
[0036] adding isopropanol to the crude glycolide to form a mixture, and heating the mixture until the crude glycolide is melted;
[0037] Let the mixed materials stand until they are separated into layers, and collect the upper layer;
[0038] Cooling, crystallizing, filtering and drying the upper layer material;
[0039] The volume of isopropanol added for every 1g of crude glycolide is less than 8mL.
[0040] The above-mentioned method for purifying glycolide is based on the principle of liquid separation method. After the glycolide crude product is mixed with isopropanol and heated, the mixed material is allowed to stand and stratification occurs. The upper material mainly includes a saturated isopropanol solution of glycolide. The upper material is collected and cooled for crystallization, filtered and dried to obtain a refined glycolide with low free acid content and high purity, which meets the application requirements for preparing degradable polymer materials. In addition, the purification yield is high, the purification method is simple, and it is beneficial to reduce production costs.
[0041] Further, in one embodiment of the present application, isopropanol is selected to mix with the glycolide crude product, and the boiling point of isopropanol is close to the melting point of glycolide. When the glycolide crude product is heated to melting, isopropanol will not boil and evaporate prematurely, so that the glycolide crude product and isopropanol can be fully dissolved. The inventor has found through research that after standing, the molten glycolide crude product will produce a stratification phenomenon with isopropanol, wherein the upper material mainly includes a saturated isopropanol solution of glycolide, and the free acid content is low, and the lower material mainly includes the molten glycolide, and at the same time, the lower material not only has a higher content of free acid, but also includes impurities such as oligomers, dust, etc. that come out with the distillation azeotropic, based on this stratification phenomenon, the inventor uses the principle of liquid separation method, and the upper material is collected separately after the mixed material is layered, and the product obtained after cooling crystallization, filtration and drying is a refined glycolide with low free acid and high purity. It can be understood that the lower material can also be collected and recycled.
[0042] The method provided in the present application uses heating and liquid separation to purify the crude glycolide. Compared with traditional purification methods such as recrystallization and distillation, the purity of the refined glycolide obtained in the present application is higher, which can reach more than 99.9%, and the free acid value can be reduced from 0.580mmol / g to less than 0.030mmol / g. The purification yield of the purification method can reach more than 50%, and the purification yield is high. Moreover, the lower layer material remaining after purification can be recycled, for example, it can be returned to the distillation kettle for secondary distillation, which can further reduce product loss. Furthermore, the purification method provided in the present application is simple and the process production process is simple. It can improve the product yield while also helping to reduce the production cost of glycolide.
[0043] Furthermore, in the process of purifying glycolide, the present application accurately controls the amount of isopropanol added to ensure a good stratification effect, effectively reduce the free acid value in the purified product, and improve the purification effect.
[0044] Furthermore, the volume ratio of isopropanol to the mass ratio of crude glycolide is (4.5-7.5) mL:1 g. The amount of isopropanol used within this range can control the amount of isopropanol added to be slightly lower than the amount required to completely dissolve the crude glycolide, which can ensure that the mixed material is separated and has a higher purification yield. It can be understood that the volume ratio of isopropanol to the mass ratio of crude glycolide can be, for example, but not limited to, 4.5 mL:1 g, 4.6 mL:1 g, 4.7 mL:1 g, 4.8 mL:1 g, 4.9 mL:1 g, 5 mL:1 g, 5.1 mL:1 g, 5.2 mL:1 g, 5.3 mL:1 g, 5.4 mL:1 g, 5.5 mL:1 g, 5.6 mL:1 g, 5.7 mL:1 g, 5.8 mL:1 g, 5.9mL:1g, 6mL:1g, 6.1mL:1g, 6.2mL:1g, 6.3mL:1g, 6.4mL:1g, 6.5mL:1g, 6.6mL:1g, 6.7m L:1g, 6.8mL:1g, 6.9mL:1g, 7mL:1g, 7.1mL:1g, 7.2mL:1g, 7.3mL:1g, 7.4mL:1g, 7.5mL:1g, etc.
[0045] In one embodiment, the heating temperature is 75°C to 85°C. Within this temperature range, the crude glycolide can be melted, and isopropanol will not evaporate due to excessive temperature, so that the crude glycolide and isopropanol can be fully mixed and dispersed, and further, it can be beneficial to promote isopropanol to dissolve glycolide, form a saturated isopropanol solution containing glycolide, and produce stratification, so as to separate the saturated isopropanol solution containing glycolide from the remaining molten glycolide crude product with high free acid content, and form an upper layer material and a lower layer material. It can be understood that the heating temperature can be, for example, but not limited to, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, etc. Preferably, the heating temperature is 83°C to 84°C.
[0046] It is understandable that the crude glycolide can be prepared by conventional methods in the art. In one embodiment, the crude glycolide is a crude product prepared by polycondensation and cracking of glycolic acid.
[0047] Further, the preparation steps of the crude glycolide product include:
[0048] Glycolic acid undergoes dehydration condensation to form polyglycolic acid oligomers;
[0049] A depolymerizing agent is added to the polyglycolic acid oligomer, and the polyglycolic acid oligomer is cracked to form a crude glycolide product.
[0050] Optionally, the deagglomerating agent may include, for example but not limited to, polyethylene glycol.
[0051] Furthermore, the conditions for dehydration condensation include: reducing the pressure to ≤3KPa; and the temperature is 180°C to 200°C.
[0052] Furthermore, the conditions for cracking include: reducing the pressure to a pressure of ≤0.2 KPa; and the temperature is 230°C to 250°C.
[0053] In one embodiment, the process of cooling, crystallizing, filtering and drying the upper material also includes a step of washing the filtered residue.
[0054] Optionally, the detergent used for washing is isopropyl alcohol.
[0055] Optionally, the number of washings is 2 to 4 times.
[0056] An embodiment of the present application further provides a refined glycolide, which is purified by the glycolide purification method in any of the above embodiments.
[0057] In one embodiment, the free acid content of the refined glycolide is ≤0.030 mmol / g; and the purity of the refined glycolide is ≥99.9%.
[0058] Glycolide raw materials suitable for preparing degradable polymer materials and meeting polymerization requirements usually require a free acid content of less than 0.030 mmol / g and a purity of more than 99.9%. The refined glycolide provided in this application meets the polymerization requirements.
[0059] One embodiment of the present application also provides an application of the refined glycolide in any of the above embodiments in the preparation of a degradable polymer material. It can be understood that the prepared degradable polymer material can be, for example, but not limited to, polyglycolic acid, poly(lactide-glycol), polycaprone, etc. Further, the above degradable polymer material can be widely used in the fields of agricultural materials, packaging materials, fracturing materials, and medical polymer materials.
[0060] An embodiment of the present application also provides a purification device, which includes a double-layer glass structure formed by a jacket, the interior of the inner layer of glass forms a tube layer of the purification device, the tube layer is used to hold materials such as crude glycolide and isopropyl alcohol, and the outer layer of glass and the inner layer of glass form an interlayer of the purification device, which is used to load heat transfer oil.
[0061] It can be understood that the outer layer of glass is provided with an oil inlet and an oil outlet connected to the interlayer, the oil inlet is located at the lower end of the outer layer of glass, and the oil outlet is located at the upper end of the outer layer of glass, the heat transfer oil is introduced from the oil inlet and discharged from the oil outlet, the oil inlet and the oil outlet are also connected to the heat transfer oil circulation machine, and the heat transfer oil circulation machine can provide pressure and control temperature.
[0062] It can be understood that the upper and lower ends of the tube layer are also provided with openings connected to the outside world, the lower end opening is used to discharge the lower layer material, and a discharge valve is also provided near the lower end opening to control the discharge of the material. The upper end opening of the tube layer can be used for adding materials, and can also be used to discharge the upper layer material, and can also be used to communicate with the nitrogen pumping device. In the process of heating the mixed material until the crude glycolide product is melted and standing to be layered, the mixed material can be protected by nitrogen to prevent the mixed material from contacting with the outside air.
[0063] It is understandable that the interior of the tube layer may also be stirred.
[0064] In one embodiment, the step of purifying glycolide using the above purification device includes:
[0065] Close the discharge valve, and add the crude glycolide to be purified and isopropanol into the tube layer in sequence to form a mixed material;
[0066] Turn on the heat transfer oil circulation machine and introduce heat transfer oil from the oil inlet;
[0067] Connect the opening at the upper end of the tube layer to a nitrogen pumping and filling device to provide nitrogen protection for the mixed material;
[0068] The mixed material is heated by heat-conducting oil until the crude glycolide product is melted;
[0069] Let the mixed materials stand until they are stratified, then open the release valve to discharge the lower layer of materials;
[0070] The upper layer material is cooled, crystallized, filtered and dried to obtain refined glycolide.
[0071] One embodiment of the present application also provides a pilot plant for preparing and purifying glycolide, which is modified based on a conventional glycolide preparation device, wherein one end of the glycolide crude product collection mechanism is connected to the solvent storage mechanism, the other end of the glycolide crude product collection mechanism is connected to the visual sensor, and the other end of the visual sensor is connected to the lower material collection mechanism and the upper material collection mechanism, respectively. When performing the purification operation, the isopropanol in the solvent storage mechanism is added to the glycolide crude product collection mechanism to form a mixed material, the glycolide crude product collection mechanism is heated until the glycolide crude product is melted, and after the mixed material is allowed to stand for stratification, the lower material is first discharged into the lower material collection mechanism, and the discharge of the lower material is monitored by the visual sensor. After the lower material is discharged, the upper material is discharged into the upper material collection mechanism, and the upper material is cooled, crystallized, filtered and dried to obtain refined glycolide.
[0072] The following is a further detailed description of the glycolide purification method, refined glycolide, and application of the present application in conjunction with specific examples and comparative examples. It is understandable that in the specific examples, unless otherwise specified, all raw materials can be sourced from common commercial sources or can be prepared by known methods. The experimental methods in the examples where specific conditions are not specified are implemented according to conventional conditions, such as the conditions described in the literature, books, or methods recommended by the manufacturer.
[0073] Example 1
[0074] Step 1: Add 600g of glycolic acid (Inokane reagent, 99%) into a 1000mL three-necked flask, reduce the pressure to 3KPa, raise the temperature to 190°C for dehydration condensation, collect the fractions, and obtain polyglycolic acid oligomers after 3 hours. The number average molecular weight of the oligomers is determined by testing the free acid value of the polyglycolic acid oligomers to reach 1000.
[0075] Step 2: Add 300 g of polyethylene glycol with a number average molecular weight of 1000 to the polyglycolic acid oligomer of step 1, replace the collecting device, raise the temperature to 240 ° C and distill under reduced pressure (pressure of 0.2 KPa) for 5 hours, the polyglycolic acid oligomer is cracked, and 270 g of the fraction is collected, i.e., crude glycolide. The free acid content is 0.580 mmol / g after testing.
[0076] Step 3: Take 8 g of the crude glycolide obtained in step 2 and add it to a glass container with a jacket, add 50 mL of dried isopropanol to form a mixture, heat it to 83°C in an anhydrous and oxygen-free environment to melt the crude glycolide, let it stand until the mixed material is stratified, discharge the lower layer material, cool the upper layer material to precipitate flaky crystals, filter and collect the residue, wash the residue with isopropanol 3 times, and then vacuum dry it at 40°C for 12 hours to obtain 5.8 g of refined glycolide.
[0077] Example 2
[0078] Step 1: Add 600g of glycolic acid (Inokane reagent, 99%) into a 1000mL three-necked flask, reduce the pressure to 3KPa, raise the temperature to 190°C for dehydration condensation, collect the fractions, and obtain polyglycolic acid oligomers after 3 hours. The number average molecular weight of the oligomers is determined by testing the free acid value of the polyglycolic acid oligomers to reach 1000.
[0079] Step 2: Add 300 g of polyethylene glycol with a number average molecular weight of 1000 to the polyglycolic acid oligomer of step 1, replace the collecting device, raise the temperature to 240 ° C and distill under reduced pressure (pressure of 0.2 KPa) for 5 hours, the polyglycolic acid oligomer is cracked, and 270 g of the fraction is collected, i.e., crude glycolide. The free acid content is 0.580 mmol / g after testing.
[0080] Step 3: Take 8 g of the crude glycolide obtained in step 2 and add it to a glass container with a jacket, add 36 mL of dried isopropanol to form a mixture, heat it to 83°C in an anhydrous and oxygen-free environment to melt the crude glycolide, let it stand until the mixed material is stratified, discharge the lower layer material, cool the upper layer material to precipitate flaky crystals, filter and collect the residue, wash the residue with isopropanol 3 times, and then vacuum dry it at 40°C for 12 hours to obtain 4.2 g of refined glycolide.
[0081] Example 3
[0082] Step 1: Add 600g of glycolic acid (Inokane reagent, 99%) into a 1000mL three-necked flask, reduce the pressure to 3KPa, raise the temperature to 190°C for dehydration condensation, collect the fractions, and obtain polyglycolic acid oligomers after 3 hours. The number average molecular weight of the oligomers is determined by testing the free acid value of the polyglycolic acid oligomers to reach 1000.
[0083] Step 2: Add 300 g of polyethylene glycol with a number average molecular weight of 1000 to the polyglycolic acid oligomer of step 1, replace the collecting device, raise the temperature to 240 ° C and distill under reduced pressure (pressure of 0.2 KPa) for 5 hours, the polyglycolic acid oligomer is cracked, and 270 g of the fraction is collected, i.e., crude glycolide. The free acid content is 0.580 mmol / g after testing.
[0084] Step 3: Take 8 g of the crude glycolide obtained in step 2 and add it to a glass container with a jacket, add 60 mL of dried isopropanol to form a mixture, heat it to 83°C in an anhydrous and oxygen-free environment to melt the crude glycolide, let it stand until the mixed material is stratified, discharge the lower layer material, cool the upper layer material to precipitate flaky crystals, filter and collect the residue, wash the residue with isopropanol 3 times, and then vacuum dry it at 40°C for 12 hours to obtain 7.0 g of refined glycolide.
[0085] Comparative Example 1
[0086] Step 1: Add 600g of glycolic acid (Inokane reagent, 99%) into a 1000mL three-necked flask, reduce the pressure to 3KPa, raise the temperature to 190°C for dehydration condensation, collect the fractions, and obtain polyglycolic acid oligomers after 3 hours. The number average molecular weight of the oligomers is determined by testing the free acid value of the polyglycolic acid oligomers to reach 1000.
[0087] Step 2: Add 300 g of polyethylene glycol with a number average molecular weight of 1000 to the polyglycolic acid oligomer of step 1, replace the collecting device, raise the temperature to 240 ° C and distill under reduced pressure (pressure of 0.2 KPa) for 5 hours, the polyglycolic acid oligomer is cracked, and 270 g of the fraction is collected, i.e., crude glycolide. The free acid content is 0.580 mmol / g after testing.
[0088] Step 3: Take 180 g of the crude glycolide obtained in step 2 and add it into a 250 mL three-necked flask with a thorny distillation column and a Kjeldahl distillation head, distill under reduced pressure at 100°C (pressure is 0.2 KPa), and collect 126 g of the fraction, which is the refined glycolide.
[0089] Comparative Example 2
[0090] Step 1: Add 600g of glycolic acid (Inokane reagent, 99%) into a 1000mL three-necked flask, reduce the pressure to 3KPa, raise the temperature to 190°C for dehydration condensation, collect the fractions, and obtain polyglycolic acid oligomers after 3 hours. The number average molecular weight of the oligomers is determined by testing the free acid value of the polyglycolic acid oligomers to reach 1000.
[0091] Step 2: Add 300 g of polyethylene glycol with a number average molecular weight of 1000 to the polyglycolic acid oligomer of step 1, replace the collecting device, raise the temperature to 240 ° C and distill under reduced pressure (pressure of 0.2 KPa) for 5 hours, the polyglycolic acid oligomer is cracked, and 270 g of the fraction is collected, i.e., crude glycolide. The free acid content is 0.580 mmol / g after testing.
[0092] Step 3: Take 30 g of the crude glycolide obtained in step 2 and recrystallize it three times using dry ethyl acetate. The amounts of ethyl acetate used for the three recrystallizations are 30 mL, 24 mL, and 18 mL, respectively. Collect the recrystallized product to obtain 16.8 g of refined glycolide.
[0093] Comparative Example 3
[0094] Step 1: Add 600g of glycolic acid (Inokane reagent, 99%) into a 1000mL three-necked flask, reduce the pressure to 3KPa, raise the temperature to 190°C for dehydration condensation, collect the fractions, and obtain polyglycolic acid oligomers after 3 hours. The number average molecular weight of the oligomers is determined by testing the free acid value of the polyglycolic acid oligomers to reach 1000.
[0095] Step 2: Add 300 g of polyethylene glycol with a number average molecular weight of 1000 to the polyglycolic acid oligomer of step 1, replace the collecting device, raise the temperature to 240 ° C and distill under reduced pressure (pressure of 0.2 KPa) for 5 hours, the polyglycolic acid oligomer is cracked, and 270 g of the fraction is collected, i.e., crude glycolide. The free acid content is 0.580 mmol / g after testing.
[0096] Step 3: Take 8 g of the crude glycolide obtained in step 2 and add it to a glass container with a jacket, add 80 mL of dried isopropanol to form a mixture, heat it to 83°C in an anhydrous and oxygen-free environment to dissolve the crude glycolide (no stratification), filter and collect the residue after cooling, wash the residue with isopropanol 3 times, and then vacuum dry it at 40°C for 12 hours to obtain 7.8 g of refined glycolide.
[0097] Comparative Example 4
[0098] Step 1: Add 600g of glycolic acid (Inokane reagent, 99%) into a 1000mL three-necked flask, reduce the pressure to 3KPa, raise the temperature to 190°C for dehydration condensation, collect the fractions, and obtain polyglycolic acid oligomers after 3 hours. The number average molecular weight of the oligomers is determined by testing the free acid value of the polyglycolic acid oligomers to reach 1000.
[0099] Step 2: Add 300 g of polyethylene glycol with a number average molecular weight of 1000 to the polyglycolic acid oligomer of step 1, replace the collecting device, raise the temperature to 240 ° C and distill under reduced pressure (pressure of 0.2 KPa) for 5 hours, the polyglycolic acid oligomer is cracked, and 270 g of the fraction is collected, i.e., crude glycolide. The free acid content is 0.580 mmol / g after testing.
[0100] Step 3: Take 8 g of the crude glycolide obtained in step 2 and add it to a glass container with a jacket, add 50 mL of dried ethanol to form a mixture, heat it to 78°C in an anhydrous and oxygen-free environment to dissolve the crude glycolide (no stratification), filter and collect the residue after cooling, wash the residue with anhydrous ethanol for 3 times, and then vacuum dry it at 40°C for 12 hours to obtain 4.8 g of refined glycolide.
[0101] The purified glycolide obtained by purification in Examples 1 to 3 and Comparative Examples 1 to 4 was subjected to purification yield calculation, and the free acid content and purity were tested. The test results are shown in Table 1 below.
[0102] Among them, the calculation formula of purification yield is:
[0103] Purification yield (%) = weight of purified glycolide / weight of crude glycolide × 100%.
[0104] The free acid test method is: accurately weigh 0.500g of the sample, dissolve it in 10mL of dimethyl sulfoxide, add 2 drops of α-naphtholphthalein indicator, and use a methanol solution containing 0.040mol / L sodium methoxide as the titrant. When the solution turns blue-green and lasts for 10 seconds, it is the titration endpoint. Calculate the sample acid value based on the volume V (mL) consumed by the titrant:
[0105] Acid value (mmol / g) = 0.040 × V (mL) / 0.500
[0106] The purity test method is: testing by GC. Figure 1 The GC test result spectrum of the purified glycolide of Example 1 is shown, and the purity results of other examples and comparative examples are shown in Table 1 below.
[0107] Table 1 Purification yield, free acid content and purity of purified glycolide
[0108]
[0109] As can be seen from Table 1, the purified glycolide obtained by Examples 1 to 3 has the characteristics of high purification yield, low free acid content, high purity, etc. Comparative Example 1 adopts the traditional distillation method for purification, and the purified glycolide has a high free acid content and low purity. Comparative Example 2 adopts the traditional recrystallization method for purification. Although the purified glycolide also has a relatively low free acid content, the purity is still inferior to that of Examples 1 to 3. In Comparative Example 3, the amount of isopropanol added is too high, and Comparative Example 4 replaces isopropanol with ethanol, but the stratification effect cannot be achieved. It is completely dissolved directly during the heating process, and the free acid content of the purified glycolide is relatively high.
[0110] The crude glycolide prepared in step 2 of Example 1 and the refined glycolide purified in step 3 were subjected to DSC test using a differential scanning calorimeter. The test conditions were: heating from room temperature to 100° C. at a rate of 1° C. / min under a nitrogen atmosphere. Figure 2 The DSC test results of the crude glycolide prepared in step 2 of Example 1 and the purified glycolide after purification in step 3 are shown. Figure 2 It can be seen that the melting point of refined glycolide is higher than that of crude glycolide and closer to the theoretical melting point of pure glycolide, which indicates that the purity of refined glycolide obtained after purification of crude glycolide is greatly improved.
[0111] like Figure 3 As shown, the purified glycolide in Example 1 after purification in step 3 is subjected to 1 HNMR test, the solvent is deuterated DMSO, δ (ppm): 5.059 (s, 4H), the compound 1 The HNMR characterization results correspond to the structural characterization results of glycolide.
[0112] The technical features of the above embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0113] The above embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the inventive concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.
Claims
1. A method for purifying glycolide, characterized in that: The following steps are involved: Providing crude glycolide to be purified; adding isopropanol to the crude glycolide to form a mixture, and heating the mixture until the crude glycolide is melted; Let it stand until stratification occurs, and collect the upper layer material; Cooling, crystallizing, filtering and drying the upper layer material; The volume of the isopropanol added per 1 g of the crude glycolide is less than 8 mL.
2. The method for purifying glycolide according to claim 1, characterized in that: The volume ratio of the isopropanol to the crude glycolide is (4.5-7.5) mL: 1 g.
3. The method for purifying glycolide according to claim 1, characterized in that: The heating temperature is 75°C to 85°C.
4. The method for purifying glycolide according to claim 3, characterized in that: The heating temperature is 83°C to 84°C.
5. The method for purifying glycolide according to any one of claims 1 to 4, characterized in that: The crude glycolide is a crude product obtained by polycondensation and cracking of glycolic acid.
6. The method for purifying glycolide according to claim 5, characterized in that: The preparation steps of the crude glycolide product include: The glycolic acid is dehydrated and condensed to form polyglycolic acid oligomers; A depolymerizing agent is added to the polyglycolic acid oligomer to crack the polyglycolic acid oligomer to form the crude glycolide.
7. The method for purifying glycolide according to claim 6, characterized in that: The conditions for dehydration condensation include: reducing the pressure to ≤3KPa; and the temperature is 180°C to 200°C.
8. The method for purifying glycolide according to claim 6, characterized in that: The conditions for cracking include: reducing the pressure to ≤0.2KPa; and the temperature is 230°C to 250°C.
9. The method for purifying glycolide according to any one of claims 1 to 4, characterized in that: The process of cooling, crystallizing, filtering and drying the upper material also includes a step of washing the filtered residue.