A kind of acid and alkali resistant high temperature adhesive tape and preparation method thereof

By using raw materials such as bisphenol A type epoxy resin and saturated styrene block copolymer, combined with emulsifier and composite curing agent, acid and alkali-resistant high-temperature tape was prepared, which solved the problem of insufficient tape strength and heat resistance, and achieved the Good acid and alkali corrosion resistance and tear resistance improve the overall performance of the tape.

CN116083022BActive Publication Date: 2024-11-22安徽谊鑫胶带有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310119125.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-15
Publication Date
2024-11-22
Estimated Expiration
2043-02-15

AI Technical Summary

Technical Problem

The existing tapes have shortcomings in terms of strength, heat resistance and acid and alkali resistance, especially in terms of high temperature resistance and acid and alkali resistance, and insufficient adhesion.

Method used

Raw materials such as bisphenol A type epoxy resin, saturated styrene block copolymer, emulsifier, composite curing agent, titanium dioxide, coupling agent and acid- and alkali-resistant filler are kneaded through plasticizing, thin-through and vacuum evacuation. The process is used to prepare acid and alkali-resistant high-temperature tape to ensure moderate rheology and viscosity of the organic carrier, and enhance the corrosion resistance, tear resistance and elasticity of the tape.

Benefits of technology

It improves the acid and alkali corrosion resistance, tear resistance and elasticity of the tape, enhances the bonding performance, ensures that it is not easy to deform and degumming under high temperature conditions, and significantly improves the mechanical strength and flame retardancy of the tape.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses an acid-base-resistant high-temperature adhesive tape and a preparation method thereof, wherein the acid-base-resistant high-temperature adhesive tape is made of the following raw materials in parts by weight: 65-75 parts of bisphenol A epoxy resin, 20-30 parts of saturated styrene block copolymer, 8-15 parts of emulsifier, 1-3 parts of modified accelerator, 2-4 parts of composite curing agent, 2-5 parts of titanium dioxide, 1-3 parts of coupling agent, 0.5-1 parts of heat-resistant agent, and 5-8 parts of acid-base corrosion-resistant filler. The present invention adopts bisphenol A epoxy resin, adjusts the rheology of the organic carrier, keeps the viscosity of the organic carrier moderate, can be fully mixed with the acid-base corrosion-resistant filler, and makes the tape have good corrosion resistance, tear resistance and elasticity. The present invention overcomes the shortcomings of the prior art, is reasonably designed, and has high social use value and application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adhesive tapes, and in particular to an acid-, alkali-, and high-temperature-resistant adhesive tape and a preparation method thereof. Background Art

[0002] Ordinary sealing packaging tape (BOPP biaxially oriented polypropylene) in daily life is an indispensable daily necessity in any enterprise, company, and personal life.

[0003] So how do you choose the quality of tape? In fact, there are two standards for the quality of tape glue in use, one is the initial adhesion, and the other is the retention, and the two are inversely proportional. Generally speaking, tapes with a viscosity lower than No. 10 have less glue coating, generally only about 20 microns, such as stationery tapes and ordinary promotional bundling tapes. The initial adhesion of normal sealing tapes is between No. 15-20, and the thickness of this tape glue is generally 22-28 microns. It is a thickness that meets the standard. However, most of the tapes on the market are mixed with impurities, so the thickness increases. In order to cover the impurities, color powder is also mixed in the glue, so the transparent tape appears egg yolk yellow and light green. This kind of tape is generally inferior.

[0004] The surface of the tape is coated with a layer of adhesive, which allows the tape to stick to objects. The earliest adhesives came from animals and plants. In the 19th century, rubber was the main component of adhesives; and now various polymers are widely used. The adhesive can stick to things because the molecules of the adhesive form bonds with the molecules of the object to be connected. This bond can firmly bond the molecules together. The ingredients of the adhesive have different polymers depending on the brand and type. This leads to the disadvantages of the tape, such as low flame retardancy, heat resistance and irritating odor.

[0005] CN104861895A discloses a high temperature resistant low viscosity vacuum bag sealing tape, which uses butyl rubber and brominated butyl rubber as base materials, polyisobutylene as a tackifier, calcium carbonate, kaolin, and talcum powder as fillers, and other additives are stirred, mixed, and extruded. The sealing tape mentioned mainly uses brominated butyl rubber, which has low strength, and the cleanability of the contact surface with the tooling after the can is out of the can cannot be guaranteed, and the applicable temperature trend is limited, and the hot pressing molding process that can be matched is limited.

[0006] CN101402764A discloses a wind-hang room temperature vacuum sealing tape and a production method thereof, which uses butyl rubber, chlorosulfonated polyethylene, polyisobutylene, calcium carbonate, 201 brominated hydroxymethyl tert-octyl phenolic resin, etc. as main matrices to prepare a vacuum sealing tape. The sealing tape mentioned uses chlorosulfonated polyethylene as a highly active rubber matrix, which affects the elasticity, high temperature resistance and air tightness of the sealant.

[0007] Therefore, in view of this, the inventor, based on his many years of rich experience in design, development and actual production in the relevant industry, has conducted research and improvement on the existing technology and its deficiencies, and provided an acid- and alkali-resistant, high-temperature-resistant, and highly adhesive tape and a preparation method thereof, in order to achieve a more practical purpose. Summary of the invention

[0008] In order to solve the problems of low strength, poor heat resistance and acid and alkali resistance of the adhesive tape mentioned in the above background technology, the present invention provides an acid and alkali resistant high temperature adhesive tape and a preparation method thereof.

[0009] In order to achieve the above object, the present invention adopts the following technical solutions:

[0010] The acid-alkali-resistant high-temperature adhesive tape is made of the following raw materials in parts by weight:

[0011] 65-75 parts of bisphenol A epoxy resin, 20-30 parts of saturated styrene block copolymer, 8-15 parts of emulsifier, 1-3 parts of modified accelerator, 2-4 parts of composite curing agent, 2-5 parts of titanium dioxide, 1-3 parts of coupling agent, 0.5-1 parts of heat-resistant agent, 5-8 parts of acid and alkali corrosion-resistant filler.

[0012] The present invention adopts bisphenol A epoxy resin, adjusts the rheological property of the organic carrier, keeps the viscosity of the organic carrier moderate, can be fully mixed with the acid and alkali corrosion resistant filler, and makes the adhesive tape have good corrosion resistance, tear resistance and elasticity.

[0013] Preferably, the modified accelerator is made from the following raw materials in parts by weight:

[0014] Accelerator MBT 35-45 parts, palmitic acid 15-25 parts, cobalt hydroxide propionate 8-10 parts, diethylenetriaminopropyltrimethoxysilane 10-20 parts, 2,4,6-tris(dimethylaminomethyl)phenol 3-5 parts.

[0015] Preferably, the emulsifier is a mixture of one or more of alkylphenol polyoxyethylene ether, isooctyl phosphate, sodium dodecylbenzene sulfonate, and sodium dodecyl diphenyl ether disulfonate;

[0016] The present invention adopts the above technical scheme, which can avoid emulsion stratification, increase the free radical concentration and branched products, make cross-linking more likely to occur and improve the conversion rate, ensure the dispersion, heat transfer and mass transfer performance of the system, improve the stability of the system, fully emulsify to reduce explosion and gel phenomenon, and improve the bonding stability of the tape;

[0017] Preferably, the composite curing agent is a compound of an amine curing agent and a hydrazide curing agent, wherein the mass ratio of the amine curing agent to the hydrazide curing agent is 1.3-1.5:2.7-3.1.

[0018] Preferably, the amine curing agent is one or more combinations of low-viscosity polyamide curing agent, N-aminoethylpiperazine, 1,3-cyclohexanedimethylamine, and N,N-dimethyldipropylenetriamine.

[0019] Preferably, the hydrazide curing agent is one or more combinations of sebacic acid dihydrazide, isophthalic acid hydrazide and succinic acid hydrazide.

[0020] The present invention adopts a compound of multiple curing agents to make up for the insufficient performance of a single curing agent. The multiple compounding produces a synergistic effect, improves the performance of the cured product, can enhance the strength of the mixed rubber, and make the high-temperature tape have good corrosion resistance, tear resistance and elasticity.

[0021] Preferably, the coupling agent is one or more combinations of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane and γ-aminopropyltrimethoxysilane.

[0022] Preferably, the heat-resistant agent is one or more combinations of α,ω-dihydroxypolydimethylsiloxane, TiO2 P25, TiO2 PF2 and polyisobutylene, which effectively improves the heat resistance of the tape and is not easy to deform or debond under long-term high temperature conditions.

[0023] Preferably, the acid and alkali corrosion resistant filler is ultrafine precipitated barium sulfate, which can greatly improve the thermal stability and acid and alkali resistance of the tape.

[0024] A method for preparing an acid- and alkali-resistant high-temperature adhesive tape further comprises the following steps:

[0025] S1: Put bisphenol A epoxy resin and saturated styrene block copolymer into an open rubber mixer and plasticize for 5-10 minutes. After plasticizing, add emulsifier, composite curing agent, modified accelerator, titanium dioxide, coupling agent, heat-resistant agent, acid and alkali corrosion-resistant filler in sequence. After each raw material is added and mixed evenly, add another raw material;

[0026] S2: After all the raw materials are added and mixed evenly, thin pass 6-8 times. During thin pass, control the roller distance of the open rubber mixer to 0.5mm and the rubber temperature ≤65℃;

[0027] S3: After thin-pass, the mixed material is transferred into a kneader for vacuum kneading. During vacuum kneading, the vacuum degree of the kneader is controlled to be ≥0.08MPa. After kneading for 25-30 minutes, the kneaded material is extruded into a tape of a certain size, that is, an acid, alkali and high temperature resistant tape is obtained.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] 1. The present invention adopts bisphenol A epoxy resin to adjust the rheological properties of the organic carrier, so that the viscosity of the organic carrier remains moderate and can be fully mixed with the acid and alkali corrosion resistant filler, so that the adhesive tape has good acid and alkali corrosion resistance, tear resistance and elasticity.

[0030] 2. The present invention adopts a composite curing agent to effectively improve the bonding performance of the organic carrier. Under the joint action of bisphenol A epoxy resin and the composite curing agent, the organic carrier is slowly volatilized in different temperature ranges to reduce the porosity of the tape mucosa and improve the density of the mucosa.

[0031] 3. The present invention adopts a compound of multiple curing agents to make up for the insufficient performance of a single curing agent. The multiple compounds produce a synergistic effect, improve the performance of the cured product, enhance the strength of the mixed rubber, and make the high-temperature tape have good corrosion resistance, tear resistance and elasticity.

[0032] 4. The present invention adds a modified accelerator after adding the composite curing agent, which accelerates the curing reaction speed of the adhesive, reduces the curing temperature, shortens the curing time, and can also improve the physical and mechanical properties of the product.

[0033] 5. The coupling agent used in the above technical solution can generate chemical bonds between linear molecules, so that the linear molecules are connected to each other to form a network structure, which can significantly improve the heat resistance, flame retardancy, solvent resistance and mechanical strength of the tape products. DETAILED DESCRIPTION

[0034] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] A kind of acid-alkali-resistant high-temperature adhesive tape, the acid-alkali-resistant high-temperature adhesive tape is made of the following raw materials in parts by weight:

[0037] 65 parts of bisphenol A epoxy resin, 20 parts of saturated styrene block copolymer, 8 parts of emulsifier, 1 part of modified accelerator, 2 parts of composite curing agent, 2 parts of titanium dioxide, 1 part of coupling agent, 0.5 parts of heat-resistant agent, and 5 parts of acid and alkali corrosion-resistant filler.

[0038] The modified accelerator is made from the following raw materials in parts by weight:

[0039] Accelerator MBT 35 parts, palmitic acid 15 parts, cobalt hydroxide propionate 8 parts, diethylenetriaminopropyltrimethoxysilane 10 parts, 2,4,6-tris(dimethylaminomethyl)phenol 3 parts.

[0040] The emulsifier is alkylphenol polyoxyethylene ether.

[0041] The composite curing agent is compounded by an amine curing agent and a hydrazide curing agent, wherein the mass ratio of the amine curing agent to the hydrazide curing agent is 1.3:2.7.

[0042] The amine curing agent is a low-viscosity polyamide curing agent.

[0043] The hydrazide curing agent is sebacic acid dihydrazide.

[0044] The coupling agent is N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane.

[0045] The heat-resistant agent is α,ω-dihydroxypolydimethylsiloxane.

[0046] The acid and alkali corrosion resistant filler is ultrafine precipitated barium sulfate.

[0047] A method for preparing an acid- and alkali-resistant high-temperature adhesive tape further comprises the following steps:

[0048] S1: Put bisphenol A epoxy resin and saturated styrene block copolymer into an open rubber mixer and plasticize for 5-10 minutes. After plasticizing, add emulsifier, composite curing agent, modified accelerator, titanium dioxide, coupling agent, heat-resistant agent, acid and alkali corrosion-resistant filler in sequence. After each raw material is added and mixed evenly, add another raw material;

[0049] S2: After all the raw materials are added and mixed evenly, thin pass 6-8 times. During thin pass, control the roller distance of the open rubber mixer to 0.5mm and the rubber temperature ≤65℃;

[0050] S3: After thin-pass, the mixed material is transferred into a kneader for vacuum kneading. During vacuum kneading, the vacuum degree of the kneader is controlled to be ≥0.08MPa. After kneading for 25-30 minutes, the kneaded material is extruded into a tape of a certain size, that is, an acid, alkali and high temperature resistant tape is obtained.

[0051] Example 2

[0052] A kind of acid-alkali-resistant high-temperature adhesive tape, the acid-alkali-resistant high-temperature adhesive tape is made of the following raw materials in parts by weight:

[0053] 68 parts of bisphenol A epoxy resin, 22 parts of saturated styrene block copolymer, 10 parts of emulsifier, 1.5 parts of modified accelerator, 3 parts of composite curing agent, 3 parts of titanium dioxide, 1.5 parts of coupling agent, 0.5 parts of heat-resistant agent, and 6 parts of acid and alkali corrosion-resistant filler.

[0054] The modified accelerator is made from the following raw materials in parts by weight:

[0055] Accelerator MBT 37 parts, palmitic acid 18 parts, cobalt hydroxide propionate 9 parts, diethylenetriaminopropyltrimethoxysilane 12 parts, 2,4,6-tris(dimethylaminomethyl)phenol 4 parts.

[0056] The emulsifier is isooctyl phosphate.

[0057] The composite curing agent is compounded by an amine curing agent and a hydrazide curing agent, wherein the mass ratio of the amine curing agent to the hydrazide curing agent is 1.3:2.8.

[0058] The amine curing agent is N-aminoethylpiperazine.

[0059] The hydrazide curing agent is isophthalic acid hydrazide.

[0060] The coupling agent is γ-aminopropyltriethoxysilane.

[0061] The heat resistant agent is TiO2 P25.

[0062] The acid and alkali corrosion resistant filler is ultrafine precipitated barium sulfate.

[0063] A method for preparing an acid- and alkali-resistant high-temperature adhesive tape further comprises the following steps:

[0064] S1: Put bisphenol A epoxy resin and saturated styrene block copolymer into an open rubber mixer and plasticize for 5-10 minutes. After plasticizing, add emulsifier, composite curing agent, modified accelerator, titanium dioxide, coupling agent, heat-resistant agent, acid and alkali corrosion-resistant filler in sequence. After each raw material is added and mixed evenly, add another raw material;

[0065] S2: After all the raw materials are added and mixed evenly, thin pass 6-8 times. During thin pass, control the roller distance of the open rubber mixer to 0.5mm and the rubber temperature ≤65℃;

[0066] S3: After thin-pass, the mixed material is transferred into a kneader for vacuum kneading. During vacuum kneading, the vacuum degree of the kneader is controlled to be ≥0.08MPa. After kneading for 25-30 minutes, the kneaded material is extruded into a tape of a certain size, that is, an acid, alkali and high temperature resistant tape is obtained.

[0067] Example 3

[0068] A kind of acid-alkali-resistant high-temperature adhesive tape, the acid-alkali-resistant high-temperature adhesive tape is made of the following raw materials in parts by weight:

[0069] 70 parts of bisphenol A epoxy resin, 25 parts of saturated styrene block copolymer, 11 parts of emulsifier, 2 parts of modified accelerator, 3 parts of composite curing agent, 3.5 parts of titanium dioxide, 2 parts of coupling agent, 1 part of heat-resistant agent, and 6.5 parts of acid and alkali corrosion-resistant filler.

[0070] The modified accelerator is made from the following raw materials in parts by weight:

[0071] Accelerator MBT 40 parts, palmitic acid 20 parts, cobalt hydroxide propionate 9 parts, diethylenetriaminopropyltrimethoxysilane 15 parts, 2,4,6-tris(dimethylaminomethyl)phenol 4 parts.

[0072] The emulsifier is a mixture of alkylphenol polyoxyethylene ether and isooctyl alcohol phosphate.

[0073] The composite curing agent is compounded by an amine curing agent and a hydrazide curing agent, wherein the mass ratio of the amine curing agent to the hydrazide curing agent is 1.4:2.9.

[0074] The amine curing agent is a combination of a low-viscosity polyamide curing agent and N-aminoethylpiperazine.

[0075] The hydrazide curing agent is a combination of sebacic acid dihydrazide and isophthalic acid hydrazide.

[0076] The coupling agent is a combination of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and γ-aminopropyltriethoxysilane.

[0077] The heat-resistant agent is a combination of α,ω-dihydroxy polydimethylsiloxane and TiO2 P25.

[0078] The acid and alkali corrosion resistant filler is ultrafine precipitated barium sulfate.

[0079] A method for preparing an acid- and alkali-resistant high-temperature adhesive tape further comprises the following steps:

[0080] S1: Put bisphenol A epoxy resin and saturated styrene block copolymer into an open rubber mixer and plasticize for 5-10 minutes. After plasticizing, add emulsifier, composite curing agent, modified accelerator, titanium dioxide, coupling agent, heat-resistant agent, acid and alkali corrosion-resistant filler in sequence. After each raw material is added and mixed evenly, add another raw material;

[0081] S2: After all the raw materials are added and mixed evenly, thin pass 6-8 times. During thin pass, control the roller distance of the open rubber mixer to 0.5mm and the rubber temperature ≤65℃;

[0082] S3: After thin-pass, the mixed material is transferred into a kneader for vacuum kneading. During vacuum kneading, the vacuum degree of the kneader is controlled to be ≥0.08MPa. After kneading for 25-30 minutes, the kneaded material is extruded into a tape of a certain size, that is, an acid, alkali and high temperature resistant tape is obtained.

[0083] Example 4

[0084] A kind of acid-alkali-resistant high-temperature adhesive tape, the acid-alkali-resistant high-temperature adhesive tape is made of the following raw materials in parts by weight:

[0085] 72 parts of bisphenol A epoxy resin, 27 parts of saturated styrene block copolymer, 13 parts of emulsifier, 2 parts of modified accelerator, 3 parts of composite curing agent, 4 parts of titanium dioxide, 2 parts of coupling agent, 1 part of heat-resistant agent, and 7 parts of acid and alkali corrosion-resistant filler.

[0086] The modified accelerator is made from the following raw materials in parts by weight:

[0087] Accelerator MBT 42 parts, palmitic acid 22 parts, cobalt hydroxide propionate 9 parts, diethylenetriaminopropyltrimethoxysilane 17 parts, 2,4,6-tris(dimethylaminomethyl)phenol 4 parts.

[0088] The emulsifier is a mixture of isooctyl phosphate and sodium dodecylbenzene sulfonate.

[0089] The composite curing agent is compounded by an amine curing agent and a hydrazide curing agent, wherein the mass ratio of the amine curing agent to the hydrazide curing agent is 1.3:2.8.

[0090] The amine curing agent is a combination of N-aminoethylpiperazine and 1,3-cyclohexanedimethylamine.

[0091] The hydrazide curing agent is a combination of sebacic acid dihydrazide and succinic acid hydrazide.

[0092] The coupling agent is a combination of γ-aminopropyltriethoxysilane and γ-aminopropyltrimethoxysilane.

[0093] The heat resistant agent is a combination of TiO2 P25 and TiO2 PF2.

[0094] The acid and alkali corrosion resistant filler is ultrafine precipitated barium sulfate.

[0095] A method for preparing an acid- and alkali-resistant high-temperature adhesive tape further comprises the following steps:

[0096] S1: Put bisphenol A epoxy resin and saturated styrene block copolymer into an open rubber mixer and plasticize for 5-10 minutes. After plasticizing, add emulsifier, composite curing agent, modified accelerator, titanium dioxide, coupling agent, heat-resistant agent, acid and alkali corrosion-resistant filler in sequence. After each raw material is added and mixed evenly, add another raw material;

[0097] S2: After all the raw materials are added and mixed evenly, thin pass 6-8 times. During thin pass, control the roller distance of the open rubber mixer to 0.5mm and the rubber temperature ≤65℃;

[0098] S3: After thin-pass, the mixed material is transferred into a kneader for vacuum kneading. During vacuum kneading, the vacuum degree of the kneader is controlled to be ≥0.08MPa. After kneading for 25-30 minutes, the kneaded material is extruded into a tape of a certain size, that is, an acid, alkali and high temperature resistant tape is obtained.

[0099] Example 5

[0100] A kind of acid-alkali-resistant high-temperature adhesive tape, the acid-alkali-resistant high-temperature adhesive tape is made of the following raw materials in parts by weight:

[0101] 75 parts of bisphenol A epoxy resin, 30 parts of saturated styrene block copolymer, 15 parts of emulsifier, 3 parts of modified accelerator, 4 parts of composite curing agent, 5 parts of titanium dioxide, 3 parts of coupling agent, 1 part of heat-resistant agent, and 8 parts of acid and alkali corrosion-resistant filler.

[0102] The modified accelerator is made from the following raw materials in parts by weight:

[0103] Accelerator MBT 45 parts, palmitic acid 25 parts, cobalt hydroxide propionate 10 parts, diethylenetriaminopropyltrimethoxysilane 20 parts, 2,4,6-tris(dimethylaminomethyl)phenol 5 parts.

[0104] The emulsifier is a mixture of alkylphenol polyoxyethylene ether, isooctyl phosphate and sodium dodecylbenzene sulfonate.

[0105] The composite curing agent is compounded by an amine curing agent and a hydrazide curing agent, wherein the mass ratio of the amine curing agent to the hydrazide curing agent is 1.5:3.1.

[0106] The amine curing agent is a combination of a low-viscosity polyamide curing agent, N-aminoethylpiperazine and 1,3-cyclohexanedimethylamine.

[0107] The hydrazide curing agent is a combination of sebacic acid dihydrazide and succinic acid hydrazide.

[0108] The coupling agent is a combination of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and γ-aminopropyltrimethoxysilane.

[0109] The heat-resistant agent is a combination of α,ω-dihydroxy polydimethylsiloxane and polyisobutylene.

[0110] The acid and alkali corrosion resistant filler is ultrafine precipitated barium sulfate.

[0111] A method for preparing an acid- and alkali-resistant high-temperature adhesive tape further comprises the following steps:

[0112] S1: Put bisphenol A epoxy resin and saturated styrene block copolymer into an open rubber mixer and plasticize for 5-10 minutes. After plasticizing, add emulsifier, composite curing agent, modified accelerator, titanium dioxide, coupling agent, heat-resistant agent, acid and alkali corrosion-resistant filler in sequence. After each raw material is added and mixed evenly, add another raw material;

[0113] S2: After all the raw materials are added and mixed evenly, thin pass 6-8 times. During thin pass, control the roller distance of the open rubber mixer to 0.5mm and the rubber temperature ≤65℃;

[0114] S3: After thin-pass, the mixed material is transferred into a kneader for vacuum kneading. During vacuum kneading, the vacuum degree of the kneader is controlled to be ≥0.08MPa. After kneading for 25-30 minutes, the kneaded material is extruded into a tape of a certain size, that is, an acid, alkali and high temperature resistant tape is obtained.

[0115] Comparative Example 1

[0116] A kind of acid-alkali-resistant high-temperature adhesive tape, the acid-alkali-resistant high-temperature adhesive tape is made of the following raw materials in parts by weight:

[0117] 65 parts of bisphenol A epoxy resin, 20 parts of saturated styrene block copolymer, 8 parts of emulsifier, 1 part of modified accelerator, 2 parts of titanium dioxide, 1 part of coupling agent, 0.5 parts of heat-resistant agent, and 5 parts of acid and alkali corrosion-resistant filler.

[0118] The modified accelerator is made from the following raw materials in parts by weight:

[0119] Accelerator MBT 35 parts, palmitic acid 15 parts, cobalt hydroxide propionate 8 parts, diethylenetriaminopropyltrimethoxysilane 10 parts, 2,4,6-tris(dimethylaminomethyl)phenol 3 parts.

[0120] The emulsifier is alkylphenol polyoxyethylene ether.

[0121] The coupling agent is N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane.

[0122] The heat-resistant agent is α,ω-dihydroxypolydimethylsiloxane.

[0123] The acid and alkali corrosion resistant filler is ultrafine precipitated barium sulfate.

[0124] A method for preparing an acid- and alkali-resistant high-temperature adhesive tape further comprises the following steps:

[0125] S1: Put bisphenol A epoxy resin and saturated styrene block copolymer into an open rubber mixer and plasticize for 5-10 minutes. After plasticizing, add emulsifier, modified accelerator, titanium dioxide, coupling agent, heat-resistant agent, acid and alkali corrosion-resistant filler in sequence. After each raw material is added and mixed evenly, add another raw material;

[0126] S2: After all the raw materials are added and mixed evenly, thin pass 6-8 times. During thin pass, control the roller distance of the open rubber mixer to 0.5mm and the rubber temperature ≤65℃;

[0127] S3: After thin-pass, the mixed material is transferred into a kneader for vacuum kneading. During vacuum kneading, the vacuum degree of the kneader is controlled to be ≥0.08MPa. After kneading for 25-30 minutes, the kneaded material is extruded into a tape of a certain size, that is, an acid, alkali and high temperature resistant tape is obtained.

[0128] Comparative Example 2

[0129] A kind of acid-alkali-resistant high-temperature adhesive tape, the acid-alkali-resistant high-temperature adhesive tape is made of the following raw materials in parts by weight:

[0130] 65 parts of bisphenol A epoxy resin, 20 parts of saturated styrene block copolymer, 8 parts of emulsifier, 1 part of modified accelerator, 2 parts of composite curing agent, 2 parts of titanium dioxide, 1 part of coupling agent, 0.5 parts of heat-resistant agent, and 5 parts of acid and alkali corrosion-resistant filler.

[0131] The modified accelerator is made from the following raw materials in parts by weight:

[0132] Accelerator MBT 35 parts, palmitic acid 15 parts, cobalt hydroxide propionate 8 parts, diethylenetriaminopropyltrimethoxysilane 10 parts, 2,4,6-tris(dimethylaminomethyl)phenol 3 parts.

[0133] The emulsifier is alkylphenol polyoxyethylene ether.

[0134] The composite curing agent is an amine curing agent, and the amine curing agent is a low-viscosity polyamide curing agent.

[0135] The coupling agent is N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane.

[0136] The heat-resistant agent is α,ω-dihydroxypolydimethylsiloxane.

[0137] The acid and alkali corrosion resistant filler is ultrafine precipitated barium sulfate.

[0138] A method for preparing an acid- and alkali-resistant high-temperature adhesive tape further comprises the following steps:

[0139] S1: Put bisphenol A epoxy resin and saturated styrene block copolymer into an open rubber mixer and plasticize for 5-10 minutes. After plasticizing, add emulsifier, composite curing agent, modified accelerator, titanium dioxide, coupling agent, heat-resistant agent, acid and alkali corrosion-resistant filler in sequence. After each raw material is added and mixed evenly, add another raw material;

[0140] S2: After all the raw materials are added and mixed evenly, thin pass 6-8 times. During thin pass, control the roller distance of the open rubber mixer to 0.5mm and the rubber temperature ≤65℃;

[0141] S3: After thin-pass, the mixed material is transferred into a kneader for vacuum kneading. During vacuum kneading, the vacuum degree of the kneader is controlled to be ≥0.08MPa. After kneading for 25-30 minutes, the kneaded material is extruded into a tape of a certain size, that is, an acid, alkali and high temperature resistant tape is obtained.

[0142] Comparative Example 3

[0143] A kind of acid-alkali-resistant high-temperature adhesive tape, the acid-alkali-resistant high-temperature adhesive tape is made of the following raw materials in parts by weight:

[0144] 65 parts of bisphenol A epoxy resin, 20 parts of saturated styrene block copolymer, 8 parts of emulsifier, 1 part of modified accelerator, 2 parts of composite curing agent, 2 parts of titanium dioxide, 1 part of coupling agent, 0.5 parts of heat-resistant agent, and 5 parts of acid and alkali corrosion-resistant filler.

[0145] The modified accelerator is made from the following raw materials in parts by weight:

[0146] Accelerator MBT 35 parts, palmitic acid 15 parts, cobalt hydroxide propionate 8 parts, diethylenetriaminopropyltrimethoxysilane 10 parts, 2,4,6-tris(dimethylaminomethyl)phenol 3 parts.

[0147] The emulsifier is alkylphenol polyoxyethylene ether.

[0148] The composite curing agent is a hydrazide curing agent, and the hydrazide curing agent is sebacic acid dihydrazide.

[0149] The coupling agent is N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane.

[0150] The heat-resistant agent is α,ω-dihydroxypolydimethylsiloxane.

[0151] The acid and alkali corrosion resistant filler is ultrafine precipitated barium sulfate.

[0152] A method for preparing an acid- and alkali-resistant high-temperature adhesive tape further comprises the following steps:

[0153] S1: Put bisphenol A epoxy resin and saturated styrene block copolymer into an open rubber mixer and plasticize for 5-10 minutes. After plasticizing, add emulsifier, composite curing agent, modified accelerator, titanium dioxide, coupling agent, heat-resistant agent, acid and alkali corrosion-resistant filler in sequence. After each raw material is added and mixed evenly, add another raw material;

[0154] S2: After all the raw materials are added and mixed evenly, thin pass 6-8 times. During thin pass, control the roller distance of the open rubber mixer to 0.5mm and the rubber temperature ≤65℃;

[0155] S3: After thin-pass, the mixed material is transferred into a kneader for vacuum kneading. During vacuum kneading, the vacuum degree of the kneader is controlled to be ≥0.08MPa. After kneading for 25-30 minutes, the kneaded material is extruded into a tape of a certain size, that is, an acid, alkali and high temperature resistant tape is obtained.

[0156] Comparative Example 4

[0157] A kind of acid-alkali-resistant high-temperature adhesive tape, the acid-alkali-resistant high-temperature adhesive tape is made of the following raw materials in parts by weight:

[0158] 65 parts of bisphenol A epoxy resin, 20 parts of saturated styrene block copolymer, 8 parts of emulsifier, 2 parts of composite curing agent, 2 parts of titanium dioxide, 1 part of coupling agent, 0.5 parts of heat-resistant agent, and 5 parts of acid and alkali corrosion-resistant filler.

[0159] The emulsifier is alkylphenol polyoxyethylene ether.

[0160] The composite curing agent is compounded by an amine curing agent and a hydrazide curing agent, wherein the mass ratio of the amine curing agent to the hydrazide curing agent is 1.3:2.7.

[0161] The amine curing agent is a low-viscosity polyamide curing agent.

[0162] The hydrazide curing agent is sebacic acid dihydrazide.

[0163] The coupling agent is N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane.

[0164] The heat-resistant agent is α,ω-dihydroxypolydimethylsiloxane.

[0165] The acid and alkali corrosion resistant filler is ultrafine precipitated barium sulfate.

[0166] A method for preparing an acid- and alkali-resistant high-temperature adhesive tape further comprises the following steps:

[0167] S1: Put bisphenol A epoxy resin and saturated styrene block copolymer into an open rubber mixer for plasticizing for 5-10 minutes. After plasticizing, add emulsifier, composite curing agent, titanium dioxide, coupling agent, heat-resistant agent, acid and alkali corrosion-resistant filler in sequence. After each raw material is added and mixed evenly, add another raw material;

[0168] S2: After all the raw materials are added and mixed evenly, thin pass 6-8 times. During thin pass, control the roller distance of the open rubber mixer to 0.5mm and the rubber temperature ≤65℃;

[0169] S3: After thin-pass, the mixed material is transferred into a kneader for vacuum kneading. During vacuum kneading, the vacuum degree of the kneader is controlled to be ≥0.08MPa. After kneading for 25-30 minutes, the kneaded material is extruded into a tape of a certain size, that is, an acid, alkali and high temperature resistant tape is obtained.

[0170] Comparative Example 5

[0171] A kind of acid-alkali-resistant high-temperature adhesive tape, the acid-alkali-resistant high-temperature adhesive tape is made of the following raw materials in parts by weight:

[0172] 65 parts of bisphenol A epoxy resin, 20 parts of saturated styrene block copolymer, 8 parts of emulsifier, 1 part of modified accelerator, 2 parts of composite curing agent, 2 parts of titanium dioxide, 1 part of coupling agent, and 5 parts of acid and alkali corrosion resistant filler.

[0173] The modified accelerator is made from the following raw materials in parts by weight:

[0174] Accelerator MBT 35 parts, palmitic acid 15 parts, cobalt hydroxide propionate 8 parts, diethylenetriaminopropyltrimethoxysilane 10 parts, 2,4,6-tris(dimethylaminomethyl)phenol 3 parts.

[0175] The emulsifier is alkylphenol polyoxyethylene ether.

[0176] The composite curing agent is compounded by an amine curing agent and a hydrazide curing agent, wherein the mass ratio of the amine curing agent to the hydrazide curing agent is 1.3:2.7.

[0177] The amine curing agent is a low-viscosity polyamide curing agent.

[0178] The hydrazide curing agent is sebacic acid dihydrazide.

[0179] The coupling agent is N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane.

[0180] The acid and alkali corrosion resistant filler is ultrafine precipitated barium sulfate.

[0181] A method for preparing an acid- and alkali-resistant high-temperature adhesive tape further comprises the following steps:

[0182] S1: Put bisphenol A epoxy resin and saturated styrene block copolymer into an open rubber mixer and plasticize for 5-10 minutes. After plasticizing, add emulsifier, composite curing agent, modified accelerator, titanium dioxide, coupling agent, acid and alkali corrosion resistant filler in sequence. After each raw material is added and mixed evenly, add another raw material;

[0183] S2: After all the raw materials are added and mixed evenly, thin pass 6-8 times. During thin pass, control the roller distance of the open rubber mixer to 0.5mm and the rubber temperature ≤65℃;

[0184] S3: After thin-pass, the mixed material is transferred into a kneader for vacuum kneading. During vacuum kneading, the vacuum degree of the kneader is controlled to be ≥0.08MPa. After kneading for 25-30 minutes, the kneaded material is extruded into a tape of a certain size, that is, an acid, alkali and high temperature resistant tape is obtained.

[0185] Comparative Example 6

[0186] A kind of acid-alkali-resistant high-temperature adhesive tape, the acid-alkali-resistant high-temperature adhesive tape is made of the following raw materials in parts by weight:

[0187] 65 parts of bisphenol A epoxy resin, 20 parts of saturated styrene block copolymer, 8 parts of emulsifier, 1 part of modified accelerator, 2 parts of composite curing agent, 2 parts of titanium dioxide, 1 part of coupling agent, and 0.5 parts of heat-resistant agent.

[0188] The modified accelerator is made from the following raw materials in parts by weight:

[0189] Accelerator MBT 35 parts, palmitic acid 15 parts, cobalt hydroxide propionate 8 parts, diethylenetriaminopropyltrimethoxysilane 10 parts, 2,4,6-tris(dimethylaminomethyl)phenol 3 parts.

[0190] The emulsifier is alkylphenol polyoxyethylene ether.

[0191] The composite curing agent is compounded by an amine curing agent and a hydrazide curing agent, wherein the mass ratio of the amine curing agent to the hydrazide curing agent is 1.3:2.7.

[0192] The amine curing agent is a low-viscosity polyamide curing agent.

[0193] The hydrazide curing agent is sebacic acid dihydrazide.

[0194] The coupling agent is N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane.

[0195] The heat-resistant agent is α,ω-dihydroxypolydimethylsiloxane.

[0196] A method for preparing an acid- and alkali-resistant high-temperature adhesive tape further comprises the following steps:

[0197] S1: Put bisphenol A epoxy resin and saturated styrene block copolymer into an open rubber mixer and plasticize for 5-10 minutes. After plasticizing, add emulsifier, composite curing agent, modified accelerator, titanium dioxide, coupling agent and heat resistant agent in sequence. After each raw material is added and mixed evenly, add another raw material;

[0198] S2: After all the raw materials are added and mixed evenly, thin pass 6-8 times. During thin pass, control the roller distance of the open rubber mixer to 0.5mm and the rubber temperature ≤65℃;

[0199] S3: After thin-pass, the mixed material is transferred to the kneading machine for vacuum kneading. During vacuum kneading, the vacuum degree of the kneading machine is controlled to be ≥0.08MPa. After kneading for 25-30 minutes, the kneaded material is extruded into a tape of a certain size, that is, an acid-alkali-resistant and high-temperature tape is obtained.

[0200] Examples 1-5 and Comparative Examples 1-6 were prepared according to the test standards, cured and formed, and relevant performance tests were performed to obtain Table 1:

[0201] Table 1

[0202]

[0203]

[0204] Compared with Example 1, Comparative Example 1 does not contain a composite curing agent; the composite curing agent in Comparative Example 2 is an amine curing agent; the composite curing agent in Comparative Example 3 is a hydrazide curing agent; no modified accelerator is added in Comparative Example 4; no heat-resistant agent is added in Comparative Example 5; and no acid- and alkali-resistant filler is added in Comparative Example 6.

[0205] The test results show that the peel strength, heat resistance and high temperature resistance of the tapes made in the comparative examples are reduced after curing, and the performance is not as good as that of the embodiments; especially the peel strength of the tape in comparative example 1 is significantly reduced after curing; the heat resistance of the tape product in comparative example 5 is significantly worse than that of the embodiments, with a large difference; and in comparative example 6, since no acid and alkali corrosion-resistant filler is added, the corrosion amount is the highest and the acid and alkali corrosion resistance is the lowest.

[0206] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A high temperature acid and alkali resistant tape, characterized in that: The acid-alkali-resistant high-temperature adhesive tape is made of the following raw materials in parts by weight: 65-75 parts of bisphenol A epoxy resin, 20-30 parts of saturated styrene block copolymer, 8-15 parts of emulsifier, 1-3 parts of modified accelerator, 2-4 parts of composite curing agent, 2-5 parts of titanium dioxide, 1-3 parts of coupling agent, 0.5-1 parts of heat-resistant agent, 5-8 parts of acid and alkali corrosion-resistant filler; The composite curing agent is compounded by an amine curing agent and a hydrazide curing agent, wherein the mass ratio of the amine curing agent to the hydrazide curing agent is 1.3-1.5:2.7-3.

1.

2. The acid-alkali-resistant high-temperature adhesive tape according to claim 1, characterized in that: The modified accelerator is made from the following raw materials in parts by weight: Accelerator MBT 35-45 parts, palmitic acid 15-25 parts, cobalt hydroxide propionate 8-10 parts, diethylenetriaminopropyltrimethoxysilane 10-20 parts, 2, 4, 6-tris(dimethylaminomethyl)phenol 3-5 parts.

3. The acid-alkali-resistant high-temperature adhesive tape according to claim 1, characterized in that: The emulsifier is a mixture of one or more of alkylphenol polyoxyethylene ether, isooctyl phosphate, sodium dodecylbenzene sulfonate, and sodium dodecyl diphenyl ether disulfonate.

4. The acid-alkali-resistant high-temperature adhesive tape according to claim 1, characterized in that: The amine curing agent is one or more combinations of low-viscosity polyamide curing agent, N-aminoethylpiperazine, 1,3-cyclohexanedimethylamine, and N,N-dimethyldipropylenetriamine.

5. The acid-alkali-resistant high-temperature adhesive tape according to claim 1, characterized in that: The hydrazide curing agent is one or more combinations of sebacic acid dihydrazide, isophthalic acid hydrazide and succinic acid hydrazide.

6. The acid-alkali-resistant high-temperature adhesive tape according to claim 1, characterized in that: The coupling agent is one or more combinations of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane and γ-aminopropyltrimethoxysilane.

7. The acid-alkali-resistant high-temperature adhesive tape according to claim 1, characterized in that: The heat-resistant agent is one or more combinations of α,ω-dihydroxy polydimethylsiloxane, TiO2 P25, TiO2 PF2 and polyisobutylene.

8. The acid-alkali-resistant high-temperature adhesive tape according to claim 1, characterized in that: The acid and alkali corrosion resistant filler is ultrafine precipitated barium sulfate.

9. A method for preparing an acid-, alkali- and high-temperature resistant adhesive tape, comprising preparing the acid-, alkali- and high-temperature resistant adhesive tape as claimed in any one of claims 1 to 8, further comprising the following steps: S1: Put bisphenol A epoxy resin and saturated styrene block copolymer into an open rubber mixer and plasticize for 5-10 minutes. After plasticizing, add emulsifier, composite curing agent, modified accelerator, titanium dioxide, coupling agent, heat-resistant agent, acid and alkali corrosion-resistant filler in sequence. After each raw material is added and mixed evenly, add another raw material; S2: After all the raw materials are added and mixed evenly, thin pass 6-8 times. During thin pass, control the roller distance of the open rubber mixer to 0.5mm and the rubber temperature ≤65℃; S3: After thin-pass, the mixed material is transferred into a kneader for vacuum kneading. During vacuum kneading, the vacuum degree of the kneader is controlled to be ≥0.08MPa. After kneading for 25-30 minutes, the kneaded material is extruded into a tape of a certain size, that is, an acid, alkali and high temperature resistant tape is obtained.