A high temperature thermal resistance coating and preparation method thereof
The multi-interface coating of Yb-doped Gd2Zr2O7 and La0.5Sr0.5FeO3 materials was prepared through the gas-liquid phase co-deposition process, which solved the problems of high infrared radiation transmittance and short life of existing thermal barrier coatings in high temperature environments. It achieves efficient infrared radiation barrier and long-life coating performance.
Patent Information
- Application Number
- CN202310023726.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-01-09
AI Technical Summary
The existing thermal barrier coating has a high transmittance to infrared radiation in high temperature environments and is easily washed and damaged during service, resulting in a decrease in reflectivity and a short life.
The multi-interface coating of Yb-doped Gd2Zr2O7 and La0.5Sr0.5FeO3 materials was prepared by gas-phase-liquid co-deposition technology. By controlling the powder particle size and powder feed rate, a columnar crystal structure and transverse microinterface were formed to improve the coating. reflectivity and bonding force.
It significantly reduces infrared radiation transmittance, improves the high-temperature insulation ability and thermal service stability of the coating, and extends the life of the coating.
Smart Images

Figure CN116083850B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of ultra-high temperature infrared radiation resistant coatings. Specifically, the present invention relates to a high temperature thermal resistance coating and a preparation method thereof, and in particular to a multi-interface ultra-high temperature and high reflectivity thermal radiation resistant coating prepared by gas-liquid co-deposition, which effectively improves the ability to inhibit infrared radiation heat transfer and the thermal service stability. Background Art
[0002] Thermal barrier coating is one of the key technologies of advanced aero engines. Its low thermal conductivity can effectively prevent the transfer of heat, reduce the operating temperature of turbine alloy blades, and extend the life of the engine. However, as the service temperature increases further, according to Boltzmann's law, when the temperature exceeds 1000℃, the heat conduction mode of thermal radiation gradually increases. In the temperature range of 1000-2000℃, the waveband of thermal radiation is mainly concentrated in the near-infrared band of 1-5 microns; the thermal barrier coating material YSZ currently used has a transmittance of up to 70% for infrared radiation of 1-5 microns within a certain thickness range, which means that in the high-temperature environment of future engines, the YSZ coating is transparent or translucent, and part of the heat is transferred to the metal substrate through the phonon effect of the ceramic material, while the other part is directly transferred to the metal substrate as infrared radiation. In order to improve the thermal insulation capacity of the coating, it is necessary to improve the barrier of thermal radiation to the coating. Therefore, if the reflection and scattering of the coating's ability to reflect and scatter near-infrared radiation can be increased, its transmittance to infrared radiation can be reduced, thereby reducing the heat penetrating the coating, the high-temperature thermal insulation capacity of the coating can be effectively improved.
[0003] At present, the commonly used coating preparation methods include atmospheric plasma spraying technology (APS), electron beam physical vapor deposition technology (EB-PVD), magnetron sputtering technology, etc. APS spraying technology is to send ceramic powder particles into a high-temperature plasma beam. The powder is heated and melted by the high-temperature beam during flight, and then hits the surface of the workpiece to be sprayed at high speed to cool, forming flat droplets. Multiple flat droplets overlap each other to form a dense coating. EB-PVD uses a high-energy electron beam to hit the target material to generate high temperature to vaporize the target material. The vaporized target atoms move upward and crystallize and grow on the surface of the cold workpiece after encountering it, forming a columnar crystal structure. Magnetron sputtering uses high-energy electron flow to impact the target material to vaporize it, and uses a magnetic field to control the flow distribution of vaporized atoms. The vaporized atoms solidify on the surface of the cold end component to form a smooth and dense coating.
[0004] At present, magnetron sputtering technology, APS technology and EB-PVD technology have been widely used to improve the reflectivity of coatings and reduce radiation transmission. For example, the ultra-smooth coating prepared by magnetron sputtering technology has significantly lower surface roughness than conventional coatings, which can effectively improve the reflectivity of infrared radiation on the coating surface and prevent more heat radiation from entering the coating (Z. Huang, Z. Wancheng, T. Xiufeng, Application of low-emissivity Pt layer on Ni
[0005] alloy to high temperature, Acta Metallurgica Sinica (English Letters) 23 (1) (2010) 1.); However, due to the harsh service environment in the engine, the coating is exposed to the impact of high-speed particles such as silicate particles and gas droplets, and the smooth surface is easily damaged, thereby affecting its ability to reflect infrared radiation. In addition, the deposition rate of magnetron sputtering technology is low, and the coating prepared is usually within 10 microns, which is difficult to effectively block the penetration of infrared radiation.
[0006] Compared with traditional single-layer coatings, multi-layer coatings prepared by APS and EB-PVD technology have one or more materials occupying one layer respectively. This method introduces a multi-layer interface within the coating system, such as the attached Figure 2 As shown, its organization is as Figure 3 As shown in the figure, at each interlayer interface, due to the different optical properties of the upper and lower layers of the interface, the reflection and scattering of infrared radiation will increase, thereby effectively reducing the infrared thermal radiation energy passing through the coating (DEWolfe, J.Singh, R.A.Miller, J.I.E.Eldridge, D.-M.Zhu, Tailored microstructure of EB-PVD 8YSZ thermal barrier coatings with low thermal conductivity and high thermal reflectivity forturbine applications, Surface and Coatings Technology 190 (1) (2005) 132-149.). However, there is a problem of weak bonding strength at the interlayer interface. During the multiple hot and cold cycles in service, cracking and peeling are more likely to occur at these interlayer interfaces, greatly reducing the coating life. Summary of the invention
[0007] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a method for preparing a high-temperature radiation-resistant coating comprising a multi-layer reflective interface and having excellent bonding strength; the coating prepared by this method has moderate thickness, low thermal conductivity, and resistance to erosion and corrosion, and can achieve the function of ultra-high temperature infrared radiation resistance and maintain stable service.
[0008] The complete technical solution of the present invention includes:
[0009] A method for producing a multi-interface ultra-high temperature and high reflectivity heat-resistant radiation coating by gas-liquid co-deposition, comprising the following steps
[0010] step:
[0011] (1) Preparation of Yb-doped Gd2Zr2O7 gadolinium zirconate material (GYbZ) and high-emissivity lanthanum strontium iron oxide La for plasma physical vapor deposition 0.5 Sr 0.5 FeO3(LSF) powder.
[0012] Among them, due to its unique energy level structure, LSF powder has the characteristics of low absorption and high reflectivity for 1-5 micron infrared band light. Compared with traditional thermal barrier coating materials such as YSZ, it can more effectively reflect infrared light and play a role in blocking radiant heat transmission. In addition, GYbZ material has good thermal stability, no phase change within 1600℃, good high temperature stability, and better thermal service performance than traditional metal coating materials. Compared with YSZ material, GYbZ material has lower thermal conductivity. As the main gas phase material of the coating, the selection of GYbZ can more effectively reduce the thermal conductivity of the coating and improve the thermal insulation performance. LSF material has high absorption characteristics in both near and mid-infrared bands, and can effectively absorb 1-6 micron infrared radiation passing through GYbZ material, greatly reducing the transmittance of the coating system. In addition, due to the large difference in the refractive index of LSF material and GYbZ material, infrared radiation will produce scattering loss at the micro interface of LSF and GYbZ. This mechanism can also reduce the infrared radiation transmittance of the coating system.
[0013] (2) Powder particle size control requires that the particle size of GYbZ be 5-15 microns and the particle size of LSF be 30-40 microns. The integrated emissivity of LSF bulk material in the 3-14 micron band is greater than 0.8.
[0014] In terms of the selection of powder particle size, it is considered that the lower the particle size, the more conducive it is to sufficient heat transfer during the movement of the powder inside the high-temperature beam. Since the heat transfer required for vaporization is higher than that for liquefaction, for the matrix material GYbZ, a powder with a small particle size and good fluidity is selected, and the particle size is smaller than that of LSF powder. For the second phase LSF material as the liquid phase sheet, its particle size is required to be slightly larger than GYbZ, but not too large, so that it can be liquefied in the beam but will not be further vaporized.
[0015] (3) The ceramic layer was prepared by PS-PVD, and the powder feeding rate was adjusted by using a dual powder feeding port to feed GYbZ and LSF powders respectively, to obtain a gas-liquid co-deposition coating with a thickness of about 200 μm. In order to control the gas-liquid co-deposition, the powder feeding rate needs to be strictly controlled, where the powder feeding rate of GYbZ powder delivered by the gas phase powder feeding port is 10-12 g / min; the powder feeding rate of LSF powder delivered by the liquid phase powder feeding port is 4-6 g / min.
[0016] The powder feeding rate affects the ratio of gas phase to liquid phase in the coating system, as well as the ability of the powder to be heated. If the LSF powder feeding rate is too high, the main structure of the coating system will be the LSF liquid phase structure, and some solid phase unmelted particles will be mixed in. If the LSF powder feeding rate is too low, the LSF powder particles will be vaporized and unable to form a horizontal interface. Therefore, controlling the powder feeding rate is a key parameter in the coating preparation process.
[0017] Traditional thermal barrier coating preparation technologies, including EB-PVD and APS, cannot achieve multiphase co-deposition, so it is difficult for technicians to think of using general coating preparation processes to achieve multi-layer micro-interface coatings. The present invention uses plasma physical vapor deposition to combine specific coating preparation process parameters with powders with specific particle size distributions to achieve the preparation of a multi-layer micro-interface infrared radiation-resistant coating. In the gas-liquid co-deposition method adopted in the present invention, during the deposition of gas-phase columnar crystals of GYbZ, liquid flat droplets of LSF are continuously deposited to form horizontal lateral micro-interfaces. Since these lateral micro-interfaces are uniformly dispersed throughout the coating, the coating can still maintain a good columnar crystal structure. Compared with multi-layer complete coating structures prepared by other methods, the coating prepared by this method has higher bonding strength and thermal cycle life. And since there is no requirement for surface roughness, the problem of decreased reflectivity caused by surface particle scouring can be avoided. Compared with the prior art, the present invention has the following advantages:
[0018] 1. Design was made in terms of component selection. First, the GYbZ material with lower near-infrared radiation emissivity and absorptivity and higher near-infrared radiation reflectivity was selected, and the LSF material with a unique energy level structure, low absorption and high reflectivity of 1-5 micron infrared band light was selected to cooperate with it, so that the prepared coating has better ability to block near-infrared thermal radiation penetration.
[0019] 2. In terms of deposition method, reasonable and optimized powder particle size, powder feeding method and powder feeding rate were carried out, and matched with the corresponding PS-PVD process parameters to achieve gas phase deposition of GYbZ materials and liquid phase deposition of LSF materials. The columnar crystal + lamellar dispersion interface of gas phase and liquid phase co-deposition has uniform thermophysical properties and ensures excellent coating adhesion.
[0020] 3. In terms of the structure of the coating, the two components are designed to form an overall columnar crystal structure with a lateral micro-interface diffuse distribution. The diffuse multi-layer interface significantly improves the coating's ability to reflect infrared thermal radiation. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram of the microstructure of the gas-liquid co-deposition coating of the present invention.
[0022] Figure 2 Schematic diagram of the multi-layer coating structure.
[0023] Figure 3 This is a diagram of the structure of a multi-layer coating. DETAILED DESCRIPTION
[0024] The following will clearly and completely describe the technical solutions in the embodiments of the present application in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only for illustration and are not intended to limit the present application.
[0025] The powder suitable for PS-PVD spraying can be prepared by any common method for preparing powder, and preferably, a spray granulation method can be used to obtain GYbZ powder with a particle size of 5-15 microns and LSF powder with a particle size of 30-40 microns.
[0026] (1) Degrease, remove rust and sandblast the metal workpiece.
[0027] (2) Preparing a metal bonding layer, preparing a NiCrAlY coating of about 50 μm thick on the surface of the clean workpiece prepared above by multi-arc ion plating; the specific steps may be: placing the high-temperature alloy workpiece pretreated in step (2) on a rotatable sample stage in a vacuum chamber, with the distance between the workpiece and the target material being about 200 mm, the temperature in the vacuum chamber being set to about 450°C, and the workpiece rotating speed being 3 rpm. When the vacuum degree in the vacuum chamber reaches 4×10 -3 The workpiece surface was ion bombarded and cleaned at pa and the surface was activated. During the coating preparation process, the reaction gas was a mixed gas of Ar and N2, with an Ar flow rate of 200sccm, a N2 flow rate of 200-400sccm, and a pressure of 1Pa. The substrate bias voltage was -80V, the arc current was 100A, and the deposition time was about 50 minutes.
[0028] 3) Use PS-PVD to prepare infrared radiation blocking coating, the specific spraying parameters are: vacuum degree of vacuum chamber 2-10mbar, static power of plasma beam 30KW-60KW, Ar carrier gas flow rate 5-20L / min, He carrier gas flow rate 10-30L / min, deposition time about 15min. Powder feeding port 1 delivers GYbZ powder, and the powder feeding amount is controlled to be 10-12g / min; powder feeding port 2 delivers LSF powder, and the powder feeding amount is controlled to be 4-6g / min.
[0029] The microstructure of the obtained vapor-liquid co-deposited coating is as follows: Figure 1 As shown, the coating maintains a columnar crystal structure as a whole, including horizontal lateral micro-interfaces in the columnar crystal structure; and is dispersed throughout the coating, with a columnar crystal diameter of about 8-10 microns and a height of about 150 microns; the lateral interface thickness is about 400nm, the width is about 2 microns, the volume fraction is about 15% of the entire coating, and the horizontal projection area is higher than 80% of the horizontal area of the coating. By selecting and setting the aforementioned process parameters, the above-mentioned optimized coating structure is obtained, so that the obtained coating has excellent infrared radiation penetration resistance, a 1100℃ thermal cycle life of 800 times, and a 1400℃ thermal conductivity of 0.9W / mK.
[0030] Comparative Example 1
[0031] Under the same conditions of other process parameters, powder feeding port 1 delivers GYbZ powder, and the powder feeding rate is controlled to be 10-12g / min;
[0032] The powder feeding port 2 conveys LSF powder, and the powder feeding amount is controlled to be 1-2 g / min. The LSF in the obtained coating cannot form horizontal lamellae, and the content is low, the infrared radiation penetration ability is reduced, and the thermal conductivity at 1400°C is 1.4 W / mK.
[0033] Comparative Example 2
[0034] Under the same conditions of other process parameters, powder feeding port 1 delivers GYbZ powder, and the powder feeding amount is controlled to be 10-12g / min; powder feeding port 2 delivers LSF powder, and the powder feeding amount is controlled to be 10-12g / min. In the obtained coating, GYbZ cannot form an obvious columnar gas phase structure, and the LSF content is high and mainly a dense liquid phase. The thermal cycle life of the coating is reduced, the thermal cycle life at 1100℃ is only 100 times, and the thermal conductivity at 1400℃ is 1.1W / mK.
[0035] The above applications are only some implementation methods of the present application. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present application, and these all belong to the protection scope of the present application.
Claims
1. A method for preparing a multi-interface ultra-high temperature and high reflectivity heat radiation resistant coating by gas-liquid co-deposition, characterized in that: The steps include: (1) Select Yb-doped Gd2Zr2O7 gadolinium zirconate (GYbZ) powder suitable for plasma physical vapor deposition process and high-emissivity lanthanum strontium iron oxide La 0.5 Sr 0.5 FeO3 is LSF powder; the particle size of the GYbZ powder is smaller than that of the LSF powder, and the integrated emissivity of the LSF material in the 3-14 micron band is greater than 0.8; the particle size of the GYbZ powder is 5-15 microns, and the particle size of the LSF powder is 30-40 microns; (2) PS-PVD equipment is used with dual powder feeding ports, wherein the gas phase powder feeding port is used to transport GYbZ powder, and the liquid phase powder feeding port is used to transport LSF powder. GYbZ and LSF powders are transported simultaneously at different powder feeding rates, wherein the powder feeding rate of the GYbZ powder is greater than the powder feeding rate of the LSF powder, and a gas-liquid co-deposited multi-interface thermal radiation-resistant ceramic coating is prepared on the surface of the workpiece; during the preparation process, the GYbZ powder is vapor deposited, and the LSF powder is liquid deposited; wherein the powder feeding rate of the GYbZ powder transported by the gas phase powder feeding port is 10-12 g / min; and the powder feeding rate of the LSF powder transported by the liquid phase powder feeding port is 4-6 g / min.
2. The method for preparing a multi-interface ultra-high temperature and high reflectivity heat-resistant radiation coating by gas-liquid co-deposition according to claim 1, characterized in that: In the step (2), the thickness of the coating obtained is 200 microns.
3. The method for preparing a multi-interface ultra-high temperature and high reflectivity heat radiation resistant coating by gas-liquid co-deposition according to claim 1, characterized in that: In the step (1), the GYbZ powder and the LSF powder are prepared by a spray granulation method.
4. The method for preparing a multi-interface ultra-high temperature and high reflectivity heat-resistant radiation coating by gas-liquid co-deposition according to claim 1, characterized in that: Before using PS-PVD equipment to prepare the coating, multi-arc ion plating was used to prepare the NiCrAlY metal bonding layer on the workpiece.
5. The method for preparing a multi-interface ultra-high temperature and high reflectivity heat-resistant radiation coating by gas-liquid co-deposition according to claim 1, characterized in that: In the step (2), the gas phase columnar crystals of GYbZ are deposited and the liquid phase flat droplets of LSF are co-deposited.
6. A multi-interface ultra-high temperature and high reflectivity heat radiation resistant coating prepared by the gas-liquid co-deposition method according to any one of claims 1 to 5, characterized in that: The coating includes a columnar crystal structure, and the columnar crystal structure of the coating includes a horizontal lateral micro-interface; the diameter of the columnar crystal is 8-10 microns and the height is 150 microns; the thickness of the lateral micro-interface is 400nm, the width is 2 microns, the volume fraction is 15% of the entire coating, and the horizontal projection area is higher than 80% of the horizontal area of the coating.
7. The coating according to claim 6, characterized in that The lateral micro-interfaces are dispersed throughout the coating, and the coating as a whole maintains a columnar crystal structure.
8. The coating according to claim 7, characterized in that The coating has a thermal cycle life of 800 times at 1100°C and a thermal conductivity of 0.9 W / mK at 1400°C.