A method for preparing catalytic cracking catalyst
By preparing ZSM-11 molecular sieve using a preset crystallization solution without templates and combining it with other components, the problems of high synthesis cost and insufficient catalytic performance of ZSM-11 molecular sieve are solved, and low-cost and efficient catalytic cracking is achieved. Catalyst preparation has the characteristics of high selectivity for low carbon olefins and low coke generation.
Patent Information
- Application Number
- CN202111324536.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-10
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-11-10
AI Technical Summary
The high synthesis cost of the existing ZSM-11 molecular sieve limits its wide application in the catalytic cracking process, and it is difficult to effectively reduce the synthesis cost and improve the selectivity of low-carbon olefins with existing technology.
By presetting the crystallization liquid as the guiding liquid, crystallizing without template agent is carried out to prepare a well-crystallized ZSM-11 molecular sieve, and combine it with components such as Y-type molecular sieve, binder and clay to form a catalytic cracking catalyst. , reduce the amount of template agent and improve the catalytic performance.
The low-cost synthesis of ZSM-11 molecular sieve is achieved, which improves the catalyst's low-carbon olefin selectivity and reduces coke generation, and has broad application prospects.
Smart Images

Figure CN116099570B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalyst preparation, and relates to a method for preparing a catalytic cracking catalyst, and in particular to a method for preparing a catalytic cracking catalyst suitable for wax residue oil processing. Background Art
[0002] In recent years, my country's finished oil production capacity has gradually exceeded demand, while there is still a large gap in low-carbon olefins such as ethylene and propylene. Catalytic cracking has the characteristics of low energy consumption and high selectivity for low-carbon olefins. It is a key technology for the transformation of refining to chemical industry. In recent years, it has become the choice of most refineries. Catalysts are its core technology. The performance of catalysts determines the product distribution and product properties of the device. However, existing catalysts have problems such as high coke production and low diene yield. Therefore, it is urgent to develop catalytic cracking catalysts that produce more low-carbon olefins and low coke production. ZSM-5 molecular sieve is a key component of catalytic cracking catalysts that produce more low-carbon olefins due to its unique pore structure and acidity. However, due to its complex Zig-Zag type tortuous pores, it has large diffusion resistance, high hydrogen transfer activity, insufficient selectivity for low-carbon olefins, and is easy to coke and deactivate. Therefore, it is urgent to develop upgraded materials to efficiently improve the selectivity of low-carbon olefins and reduce coke production.
[0003] ZSM-11 zeolite belongs to the tetragonal system and has a two-dimensional pore structure. It is an important adsorbent and a good shape-selective catalyst. It belongs to the pentasil family with ZSM-5 zeolite and has the same form of sheet structure. Unlike ZSM-5, the adjacent layers are not related by the symmetry center, but by the mirror plane, which produces a ten-membered ring straight channel parallel to the a direction and the b direction, and it is easy to produce impurities during the synthesis process. Compared with the complex Zig-Zag type tortuous channel of ZSM-5, the unique two-dimensional straight channel of ZSM-11 makes the diffusion resistance of hydrocarbon molecules inside it relatively small, which is conducive to the timely diffusion of small molecular olefins out of the channel, reducing the possibility of side reactions, thereby improving the selectivity of low-carbon olefins and reducing coke.
[0004] Patent CN201510685830.7 discloses a fluidized bed catalyst for preparing olefins and aromatics and its application, which is characterized in that P, Zn, Ga, Cr, Mo, rare earth, Fe or Co are added during the preparation of the catalyst containing ZSM-11 molecular sieve, and is applied to the catalytic cracking process of naphtha to increase the yield of ethylene + propylene + aromatics, but there is no mention of reducing the cost of ZSM-11.
[0005] Patent CN201310072027.7 discloses a catalyst for catalytic cracking of heavy oil, characterized in that a ZSM-11 molecular sieve modified with phosphorus and transition metal elements or a eutectic molecular sieve of modified ZSM-5 and ZSM-11 is added during the preparation of the catalyst, which can promote the catalytic conversion of heavy oil, increase the olefin content of liquefied gas and reduce the benzene content of gasoline, and the catalyst has good stability, but there is no mention of reducing the cost of ZSM-11.
[0006] Li Yang et al., in the study of ZSM-11 molecular sieve for heavy oil catalytic cracking process, compared the heavy oil cracking performance of ZSM-5 molecular sieve and ZSM-11 molecular sieve catalysts. The results showed that ZSM-11 molecular sieve can improve the octane number of gasoline while reducing gasoline loss and reducing dry gas and coke yields. However, there is no mention of reducing the cost of ZSM-11.
[0007] At present, the main factor limiting the widespread application of ZSM-11 molecular sieve is the high synthesis cost. Therefore, it is necessary to reduce the amount of template used in the synthesis process to achieve low-cost synthesis of ZSM-11.
[0008] Patent CN201710792799.6 discloses a method for preparing large / mesoporous zeolite molecular sieves by seed induction. Zeolite molecular sieve seeds are first prepared using an organic template agent, and then a small amount of seeds are added to the synthesis liquid of the zeolite molecular sieve. Through simple high-temperature hydrothermal crystallization, uniform-sized meso / large-pore zeolite ZSM-11 molecular sieves can be obtained. The seeds are first synthesized by long-term crystallization using an organic silicon source template method, and the seed preparation cost is high.
[0009] Patent CN201811583072.8 discloses a method for synthesizing a surface aluminum-rich ZSM-23 molecular sieve, which is characterized in that a molecular sieve gel is prepared and pre-crystallized at the initial stage of synthesis to form a large number of molecular sieve crystal nuclei with a relatively high silicon-aluminum ratio; then a synthetic gel with a low silicon-aluminum ratio and no template is added thereto, and after 1 to 96 hours, it can be rapidly crystallized to form an aluminum-rich ZSM-23 molecular sieve with a surface silicon-aluminum ratio of 10 to 80. It first synthesizes molecular sieve crystal nuclei with a high silicon-aluminum ratio, and then mixes and crystallizes them with a low silicon-aluminum ratio gel at a ratio of 0.6-0.7. The proportion of pre-crystallization liquid containing the template is high, the reduction in the amount of the template is limited, and the silicon source utilization rate of this method is low.
[0010] Patent CN101531376A discloses a microwave synthesis process for ZSM-11, which is characterized by replacing traditional hydrothermal heating with microwave radiation heating, and by pre-setting crystal seeds, the nucleation rate and crystal growth rate are significantly accelerated, and the crystallization time is greatly shortened. However, microwave radiation heating does not have a certain equipment foundation nationwide, and its industrial application is limited. Moreover, although the use of crystal seeds can accelerate the purification rate, the crystal seeds are pure ZSM-11 molecular sieves, which will increase the synthesis cost.
[0011] Patent CN201911079671.0 discloses millimeter-scale microspherical molecular sieves and their preparation methods, which are characterized in that the initial crystallization liquid formed after the raw materials containing the template and the silicon source are crystallized is mixed with a spheroidizing agent; and then hydrothermal crystallization is performed to form a spherical molecular sieve precursor. The first step of crystallization is a mixed crystallization process of an aluminum source, a template and a silicon source, or a mixed crystallization process of a template and a silicon source, and the crystallization conditions are a temperature of 90-200°C and a time of 20-140 minutes. However, this technology only adds a spheroidizing agent to the initial crystallization liquid, changes the molecular sieve particles, and its crystallization system does not change, and the amount of template cannot be reduced, and the synthesis cost is high.
[0012] In recent years, many scholars have devoted themselves to the research of catalytic cracking catalysts, but each preparation method has the disadvantages of poor coke selectivity and ethylene + propylene selectivity and high production cost. Therefore, it is necessary to provide a preparation method of catalytic cracking catalysts with excellent performance and low cost. Summary of the invention
[0013] In order to solve the above technical problems, the purpose of the present invention is to provide a method for preparing a catalytic cracking catalyst, which can solve the problem of high preparation cost of ZSM-11 molecular sieve in the prior art. By pre-setting a crystallization liquid as a guide liquid, a well-crystallized ZSM-11 molecular sieve can be obtained by crystallizing for a period of time under template-free conditions, which is used as a catalytic cracking catalyst to improve coke selectivity and increase ethylene + propylene selectivity.
[0014] To achieve the above object, the present invention provides a method for preparing a catalytic cracking catalyst, the preparation method comprising the following steps:
[0015] S1. Synthesize a ZSM-11 initial gel mixture according to a molar ratio of 0.12-0.2M2O: 0.005-0.01Al2O3: 1SiO2: 10-30H2O: 0.3-0.8(TBA)2O, and crystallize the gel mixture for 2-11 hours to obtain a pre-crystallization solution; wherein M is an alkali metal, Al2O3 is an aluminum source, SiO2 is a silicon source, and (TBA)2O is a template;
[0016] S2, in the same proportion as the pre-crystallization solution, without adding a template, a silicon source, an aluminum source, an alkali source and water are prepared into a ZSM-11 initial gel solution;
[0017] S3, adding the pre-crystallization solution in step S1 to the initial gel solution in step S2 to obtain a gel mixture, and further crystallizing to obtain a ZSM-11 molecular sieve crystallization solution;
[0018] S4, separating, cooling, filtering and washing the ZSM-11 molecular sieve crystallization liquid, and modifying the obtained filter cake by ammonium salt exchange and roasting to obtain ZSM-11 molecular sieve;
[0019] S5. Based on 100 parts of the dry basis weight of the catalyst, 15-40 parts of ZSM-11 molecular sieve, 5-15 parts of Y-type molecular sieve, 5-15 parts of binder, 35-75 parts of clay and water are slurried, spray-formed, and calcined to obtain a catalytic cracking catalyst. The molar ratio of the components in the ZSM-11 initial gel mixture in step S1 of the preparation method of the catalytic cracking catalyst of the present invention is preferably 0.14-0.18M2O: 0.005-0.01Al2O3: 1SiO2: 15-25H2O: 0.4-0.7(TBA)2O; the molar ratio of Si to Al in the ZSM-11 initial gel mixture is 50-100, and the molar ratio of Si to Al here represents the molar ratio of Si atoms to Al atoms.
[0020] In the preparation method of the catalytic cracking catalyst of the present invention and the synthesis method of the ZSM-11 molecular sieve, the alkali metal is preferably Na, K or Li.
[0021] In the method for preparing the catalytic cracking catalyst of the present invention and the method for synthesizing the ZSM-11 molecular sieve, the silicon source preferably includes at least one of alkaline silica sol, silica gel and water glass.
[0022] In the preparation method of the catalytic cracking catalyst of the present invention and the synthesis method of the ZSM-11 molecular sieve, the aluminum source preferably includes at least one of aluminum chloride, aluminum sulfate and aluminum nitrate.
[0023] In the preparation method of the catalytic cracking catalyst of the present invention and the synthesis method of the ZSM-11 molecular sieve, the template agent is preferably a tetrabutylammonium template agent.
[0024] In the preparation method of the catalytic cracking catalyst of the present invention and the synthesis method of the ZSM-11 molecular sieve, the tetrabutylammonium template preferably includes at least one of tetrabutylammonium bromide and tetrabutylammonium hydroxide.
[0025] In the method for preparing the catalytic cracking catalyst of the present invention, in step S1, in the method for synthesizing the ZSM-11 molecular sieve, the crystallization conditions are preferably: temperature 150° C.-170° C., time 2-4 hours.
[0026] In the preparation method of the catalytic cracking catalyst of the present invention, in step S3, in the synthesis method of the ZSM-11 molecular sieve, the crystallization conditions are preferably: temperature 150° C.-170° C., time 24-72 hours, preferably 48-60 hours.
[0027] In the preparation method of the catalytic cracking catalyst of the present invention, in step S3, in the synthesis method of the ZSM-11 molecular sieve, the addition amount of the pre-crystallization liquid is 10wt% to 50wt%, preferably 25wt% to 50wt% of the ZSM-11 initial gel solution.
[0028] The preparation method of the catalytic cracking catalyst described in the present invention, in step S4, in the synthesis method of the ZSM-11 molecular sieve, the ammonium salt exchange modification of the ZSM-11 molecular sieve is carried out in the following manner: at least one of ammonium chloride, ammonium nitrate and ammonium sulfate is exchanged with the ZSM-11 molecular sieve and filtered 1-3 times until Na2O is less than 0.5wt%.
[0029] In the preparation method of the catalytic cracking catalyst described in the present invention, in step S5, preferably, ZSM-5 molecular sieve, metal modification element B, and phosphorus-containing substance are also added; based on 100 parts of the dry basis mass of the catalyst, 15-40 parts of ZSM-11 molecular sieve, 0-15 parts of ZSM-5 molecular sieve, 5-15 parts of Y-type molecular sieve, 5-15 parts of binder, 35-75 parts of clay, 0-3 parts of metal modification element B, and 0-10 parts of phosphorus-containing substance (calculated as P2O5) are slurried with water, spray-formed, and calcined to obtain a catalytic cracking catalyst.
[0030] In the preparation method of the catalytic cracking catalyst described in the present invention, in step S5, preferably, the catalyst has a ratio of: based on 100 parts of the dry basis mass of the catalyst, 18-28 parts of ZSM-11 molecular sieve, 3-8 parts of ZSM-5 molecular sieve, 5-10 parts of Y-type molecular sieve, 7-15 parts of binder, 40-50 parts of clay, 1-2 parts of metal modification element B, and 4-8 parts of phosphorus-containing substances (calculated as P2O5).
[0031] In the method for preparing the catalytic cracking catalyst of the present invention, in step S5, the ZSM-11 molecular sieve may be at least one of the ZSM-11 molecular sieve prepared in step S4 and a modified ZSM-11 molecular sieve. The modification method of the modified ZSM-11 molecular sieve is as follows: the concentration of the ZSM-11 molecular sieve slurry obtained in step S4 is adjusted to a solid content of 80 to 400 g / L, 0.3% to 5% of the weight of the molecular sieve is added, preferably 0.5-2.5% by weight of a modified metal element A salt for exchange modification, the metal modified element A includes at least one chloride or nitrate of Ag, Zn, and rare earth elements, the exchange temperature is 0 to 100° C., and the exchange time is 0.1 to 1.5 hours, and then 0-5% of the weight of the molecular sieve (in terms of P2O5), preferably 1-3% by weight, is added with stirring, the phosphorus-containing substance includes at least one of phosphoric acid, ammonium phosphate, ammonium hydrogen phosphate and diammonium phosphate, preferably ammonium phosphate, the reaction temperature is 0 to 100° C., the reaction time is 0.1 to 1 hour, and the modified ZSM-11 molecular sieve is obtained by filtering, washing with water, and roasting, or without filtering, washing with water, and roasting.
[0032] In the method for preparing the catalytic cracking catalyst of the present invention, in step S5, the ZSM-5 molecular sieve includes at least one of HZSM-5, Ag, Zn, Fe, rare earth, and P-modified ZSM-5.
[0033] In the method for preparing the catalytic cracking catalyst of the present invention, in step S5, the Y-type molecular sieve includes at least one of USY, HY, REY, REHY, and REUSY, preferably USY and REUSY.
[0034] In the method for preparing the catalytic cracking catalyst of the present invention, in step S5, the binder includes at least one of aluminum sol, acidified pseudo-boehmite, acidic silica sol and phosphate aluminum sol.
[0035] In the method for preparing the catalytic cracking catalyst of the present invention, in step S5, the clay comprises at least one of kaolin, halloysite, porphyrite, diatomite and vesicle stone.
[0036] In the method for preparing the catalytic cracking catalyst of the present invention, in step S5, the metal modification element B used in the catalyst preparation includes at least one of the elements Ag, Zn, Fe, La, Ce, etc., and the addition form thereof can be chloride or nitrate.
[0037] In the method for preparing the catalytic cracking catalyst of the present invention, in step S5, the phosphorus-containing substance used for preparing the catalyst includes at least one of phosphoric acid, ammonium phosphate, ammonium hydrogen phosphate and diammonium phosphate, preferably phosphoric acid.
[0038] Compared with the prior art, the present invention has the following advantages and effects:
[0039] (1) The present invention first forms a crystal structure unit, and uses a pre-crystallization liquid as a guide liquid to induce crystallization in the absence of a template to obtain a well-crystallized ZSM-11 molecular sieve. This method can greatly reduce the amount of template used and avoid the addition of expensive seed crystals, which is beneficial to reducing the synthesis cost of the ZSM-11 molecular sieve and is beneficial to environmental protection.
[0040] (2) By adding a pre-crystallization liquid to the initial gel solution of ZSM-11, not only can the amount of template used in the ZSM-11 molecular sieve be greatly reduced, but also because the gel system and the pre-crystallization liquid system have the same ratio of alkali, silicon source, aluminum source, and water, it is easy to form a uniform crystallization system, which can achieve rapid synthesis of the molecular sieve while ensuring its high crystallinity, greatly shortening the pre-crystallization time.
[0041] (3) The ZSM-11 molecular sieve prepared by the method of the present invention has a higher silicon-aluminum ratio, and the catalytic cracking catalyst containing the ZSM-11 molecular sieve prepared has the characteristics of high selectivity for light olefins and low coke generation, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is the X-ray diffraction (XRD) spectrum of ZSM-11 molecular sieve A-11-3 synthesized in Example 3. DETAILED DESCRIPTION
[0043] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.
[0044] Some of the raw materials used in the examples are:
[0045] The sample of ZSM-11 purchased from the standard market.
[0046] NaOH, KOH, Al2(SO4)3, (TBA)2O, ammonium chloride, ammonium nitrate, ammonium sulfate, silver nitrate, zinc nitrate, zinc chloride, lanthanum nitrate, lanthanum chloride, ammonium phosphate, diammonium hydrogen phosphate, monoammonium phosphate, and phosphoric acid are reagents.
[0047] Alkaline silica sol (SiO2 content 30%, model JN-30), acidic silica sol (SiO2 content 30%, model ZA-30), water glass, alumina sol (Al2O3 content 21.7%), kaolin, halloysite, pseudo-boehmite, REUSY (RE2O3 content 2.4%) and ZSM-5 (silicon to aluminum ratio 42) are industrial products.
[0048] The test items are:
[0049] (1) X-ray diffraction
[0050] The X-ray diffractometer used for the determination of the physical phase and relative crystallinity of the ZSM-11 molecular sieve is a Panalytical X'Pert Powder diffractometer, with a test voltage of 40 kV, a test current of 40 mA, and a test range of 5-50°.
[0051] (2) Crystallinity
[0052] Place the dried, ground and dispersed sample on the glass test window, flatten the sample with a glass slide, and scan it in the instrument. Use Highscore software to calculate the relative crystallinity of the sample. The calculation formula is as follows:
[0053] Relative crystallinity of sample % = (∑ characteristic peak area of sample / mean value) / (∑ characteristic peak area of standard sample / mean value) × relative crystallinity of standard sample.
[0054] (3) Micro-evaluation
[0055] The catalyst was pre-treated at 800°C and 100% steam for 17 hours, the reaction temperature was 570°C, the catalyst-oil ratio was 9, and the raw material oil was Dushanzi wax oil.
[0056] Example 1
[0057] The preparation method of the catalytic cracking catalyst provided in this embodiment comprises the following steps:
[0058] Step 1: Synthesize ZSM-11 molecular sieve pre-crystallization solution:
[0059] According to the components and molar ratio of 0.18M2O:0.01Al2O3:1SiO2:18H2O:0.45(TBA)2O, wherein M represents alkali metal, the raw material of M2O is the alkali source KOH, the raw material of Al2O3 is the aluminum source Al2(SO4)3, the raw material of SiO2 is the silicon source alkaline silica sol, (TBA)2O represents the template, and this embodiment uses tetrabutylammonium hydroxide as the template, configured into a ZSM-11 initial gel mixture, and the Si / Al of the gel mixture is 50 (molar ratio).
[0060] The gel mixture was stirred at 25° C. for 1-2 hours until it was uniform, and then the gel mixture was transferred to a crystallization kettle and crystallized at 160° C. for 4 hours to obtain the pre-crystallization solution required for the next step of synthesis.
[0061] Step 2: Synthesize ZSM-11 molecular sieve crystallization solution:
[0062] According to the same components and proportions as the ZSM-11 initial gel mixture in step 1, raw materials silicon source, aluminum source, alkali source and water are added, and a ZSM-11 initial gel solution is prepared without adding a template, and then the pre-crystallization liquid prepared in step 1 is added as a guide liquid, the mass ratio of the guide liquid to the ZSM-11 initial gel solution is 1:2, stirred at room temperature for 1-2 hours until uniform and transferred to a crystallization kettle, crystallized at 170°C for 48 hours to obtain a ZSM-11 molecular sieve crystallization liquid.
[0063] Step 3: Preparation of HZSM-11 molecular sieve:
[0064] The ZSM-11 molecular sieve crystallization liquid obtained in step 2 is separated by vacuum filtration, cooled, filtered, and washed until neutral. The filter cake is exchanged three times by adding 30% by weight of ammonium nitrate, the filter cake is dried at 100°C for 4 hours, and calcined at 550°C for 1.5 hours to obtain HZSM-11, which is recorded as A-11-1.
[0065] Step 4: Preparation of modified ZSM-11 molecular sieve:
[0066] The HZSM-11 prepared in step 3 was adjusted to a solid content of 150 g / L, and 2.2 wt % silver nitrate (Ag) was added for exchange modification at room temperature for 30 min. The modified ZSM-11 molecular sieve was obtained by filtration and calcination at 550° C. for 2 h, and was recorded as P-11-1.
[0067] Step 5, preparing catalytic cracking catalyst:
[0068] The ZSM-11 molecular sieve P-11-1 from step four is slurried with water in the ratio of dry basis ZSM-11: ZSM-5: REUSY: aluminum sol: acidic silica sol: halloysite: ferric chloride (calculated as Fe2O3): phosphoric acid (calculated as P2O5) = 20:8:8:7:10:39.5:1.5:6 to form a slurry with a solid content of 40%, and then spray-formed and calcined at 470°C for 30 minutes to obtain catalytic cracking catalyst C-1.
[0069] Example 2
[0070] The preparation method of the catalytic cracking catalyst provided in this embodiment comprises the following steps:
[0071] Step 1, according to the molar ratio of 0.14M2O: 0.00625Al2O3: 1SiO2: 20H2O: 0.37(TBA)2O, wherein M represents alkali metal, the raw material of M2O is the alkali source NaOH, the raw material of Al2O3 is the aluminum source Al2(SO4)3, the raw material of SiO2 is the silicon source alkaline silica sol, (TBA)2O represents the template, and this embodiment uses tetrabutylammonium hydroxide as the template to form a ZSM-11 initial gel mixture, and the Si / Al of the gel mixture is 80 (molar ratio).
[0072] The gel mixture was crystallized at 150° C. for 2 hours by a conventional hydrothermal synthesis method to directly synthesize a ZSM-11 molecular sieve pre-crystallization solution.
[0073] Step 2: Add the pre-crystallization liquid synthesized in step 1 to the ZSM-11 initial gel solution with the same proportion and silicon-aluminum ratio (Si / Al=100) as a guiding liquid, the mass ratio of the guiding liquid to the initial gel solution is 1:3, stir until uniform at room temperature, transfer the gel mixture to a crystallization kettle, and crystallize at 150°C for 60 hours to obtain a ZSM-11 molecular sieve crystallization liquid.
[0074] Step 3: Preparation of HZSM-11 molecular sieve:
[0075] The ZSM-11 molecular sieve crystallization liquid obtained in step 2 is separated by vacuum filtration, cooled, filtered, and washed until neutral. The filter cake is exchanged once with 40% by weight of ammonium nitrate, the filter cake is dried at 100°C for 4.5h, and calcined at 550°C for 1.5h to obtain HZSM-11, which is recorded as A-11-2.
[0076] Step 4: Preparation of modified ZSM-11 molecular sieve:
[0077] The HZSM-11 prepared in step 3 was adjusted to a solid content of 150 g / L, and 0.5 wt% zinc nitrate (calculated as Zn) was added for exchange modification at room temperature for 45 minutes. Then, 2.8 wt% diammonium hydrogen phosphate (calculated as P2O5) was added under stirring, and the reaction was carried out at room temperature for 25 minutes. The modified ZSM-11 molecular sieve was obtained by filtration, 1-fold water washing, and calcination at 550°C for 3 hours, which was recorded as P-11-2.
[0078] Step 5, preparing catalytic cracking catalyst:
[0079] The ZSM-11 molecular sieve P-11-2 from step four is slurried with water in the ratio of dry basis ZSM-11: ZSM-5: REUSY: aluminum sol: acidic silica sol: halloysite: ferric chloride (calculated as Fe2O3): phosphoric acid (calculated as P2O5) = 21:6:7:8:8:43.2:1.8:5 to form a slurry with a solid content of 42%, and then spray-formed and calcined at 500°C for 25 minutes to obtain a catalytic cracking catalyst C-2.
[0080] Example 3
[0081] The preparation method of the catalytic cracking catalyst provided in this embodiment comprises the following steps:
[0082] Step 1, according to the molar ratio of 0.12M2O:0.005Al2O3:1SiO2:25H2O:0.72(TBA)2O, wherein M represents alkali metal, the raw material of M2O is the alkali source NaOH, the raw material of Al2O3 is the aluminum source Al2(SO4)3, the raw material of SiO2 is the silicon source water glass, (TBA)2O represents the template, and this embodiment uses tetrabutylammonium hydroxide as the template to form a ZSM-11 initial gel mixture, and the Si / Al of the gel mixture is 100 (molar ratio).
[0083] The gel mixture was crystallized at 170° C. for 2 hours by a conventional hydrothermal synthesis method to directly synthesize a ZSM-11 molecular sieve pre-crystallization solution with Si / Al=100.
[0084] Step 2: Add the pre-crystallization liquid synthesized in step 1 to the ZSM-11 initial gel solution with the same proportion and silicon-aluminum ratio (Si / Al=100) as a guiding liquid, the mass ratio of the guiding liquid to the initial gel solution is 1:3, stir until uniform at room temperature, transfer the gel mixture to a crystallization kettle, and crystallize at 160°C for 54 hours to obtain a ZSM-11 molecular sieve crystallization liquid.
[0085] Step 3: Preparation of HZSM-11 molecular sieve:
[0086] The ZSM-11 molecular sieve crystallization liquid obtained in step 2 is separated by vacuum filtration, cooled, filtered, and washed until neutral. The filter cake is exchanged once with 40% by weight of ammonium chloride, the filter cake is dried at 100°C for 4.5h, and calcined at 550°C for 1.5h to obtain HZSM-11, which is recorded as A-11-3.
[0087] Step 4: preparing catalytic cracking catalyst:
[0088] The ZSM-11 molecular sieve A-11-3 in step three is slurried with water in the ratio of dry basis ZSM-11: ZSM-5: REUSY: aluminum sol: acidic silica sol: halloysite: silver nitrate (Ag): phosphoric acid (P2O5) = 22:5:6:6:13:40:1:7 to form a slurry with a solid content of 38%, and then spray-formed and calcined at 450°C for 45 minutes to obtain catalytic cracking catalyst C-3.
[0089] Example 4
[0090] Preparation of catalytic cracking catalyst:
[0091] The ZSM-11 molecular sieve A-11-1 from step three of Example 1 was slurried with water in the ratio of dry basis ZSM-11: ZSM-5: REUSY: aluminum sol: acidified pseudo-boehmite: kaolin: zinc chloride (in terms of ZnO): phosphoric acid (in terms of P2O5) = 25:3:9:8:11:34.8:1.2:8 to prepare a slurry with a solid content of 35%, and the slurry was spray-formed and calcined at 450°C for 40 minutes to obtain a catalytic cracking catalyst C-4.
[0092] Example 5
[0093] Preparation of catalytic cracking catalyst:
[0094] The ZSM-11 molecular sieve P-11-2 from step four of Example 2 and the ZSM-11 molecular sieve A-11-3 from step three of Example 3 were mixed with water in the ratio of dry basis P-11-2: A-11-3: REUSY: alumina sol: acidified pseudo-boehmite: kaolin: ferric nitrate (calculated as Fe2O3): phosphoric acid (calculated as P2O5) = 8:18:6:9:8:43:2:6 to prepare a slurry with a solid content of 39%, and the mixture was spray-formed and calcined at 460°C for 35 minutes to obtain a catalytic cracking catalyst C-5.
[0095] Comparative Example 1
[0096] This comparative example adopts a method for preparing a catalytic cracking catalyst of ZSM-5 molecular sieve, which comprises the following steps:
[0097] The catalytic cracking catalyst DB-C1 was prepared by mixing dry basis ZSM-5:REUSY:alumina sol:acidified pseudo-boehmite:kaolin in a ratio of 25:10:10:10:45 with water to prepare a slurry with a solid content of 30%. The slurry was spray-formed and calcined at 450°C for 50 minutes to obtain a catalytic cracking catalyst.
[0098] Comparative Example 2
[0099] Step 1: This comparative example adopts the conventional preparation method of ZSM-11 molecular sieve:
[0100] According to the molar ratio of 0.16Na2O:0.005Al2O3:1SiO2:18H2O:0.42(TBA)2O, the raw materials were added in sequence and stirred until a uniform gel was obtained. The gel mixture was transferred to a crystallization kettle and crystallized at 160°C for 75 hours. The mixture was filtered and washed until neutral. The filter cake was exchanged twice with 25% by weight of ammonium sulfate. The filter cake was dried at 100°C for 3 hours and calcined at 550°C for 2 hours to obtain HZSM-11, which was recorded as DB-Z11.
[0101] Step 2, a method for preparing a catalytic cracking catalyst, comprising the following steps:
[0102] The ZSM-11 molecular sieve DB-11 from step 1 is slurried with water in a ratio of dry basis ZSM-11: REUSY: alumina sol: acidified pseudo-boehmite: kaolin = 27:9:10:9:45 to form a slurry with a solid content of 31%, and then spray-formed and calcined at 460°C for 40 minutes to obtain a catalytic cracking catalyst DB-C2.
[0103] Table 1 Analysis results of molecular sieve physical and chemical properties
[0104] Molecular sieve number <![CDATA[Na2O]]> <![CDATA[P2O5]]> Ag Zn <![CDATA[La2O3]]> Si / Al Relative crystallinity retention rate, % A-11-1 0.15 48 83.7 P-11-1 0.09 1.96 90.1 A-11-2 0.23 77 86.3 P-11-2 0.19 2.51 0.48 94.6 A-11-3 0.20 100 86.9 P-11-3 0.16 1.80 3.43 92.8 DB-Z11 0.17 83.2
[0105] Note: Relative crystallinity retention rate = relative crystallinity (aged sample) / relative crystallinity (fresh sample) × 100%
[0106] Aging conditions: 800℃, 100% water vapor for 17 hours
[0107] The results in Table 1 show that the ZSM-11 molecular sieve prepared by the present invention has the advantages of low template dosage, high silicon source utilization rate and good hydrothermal stability.
[0108] Table 2 shows the evaluation results of the catalyst micro-reaction obtained in Examples 1 to 5 and Comparative Example 1, and the gasoline properties are shown in Table 3. The evaluation conditions are: the raw oil is Dushanzi wax oil, the catalyst-to-oil ratio is 9, and the reaction temperature is 570° C. The evaluation results show that the catalytic cracking catalyst prepared by the present invention has the characteristics of low coke generation and high ethylene + propylene yield.
[0109] Table 2 ACE micro-antibody evaluation results
[0110]
[0111]
[0112] The results in Table 2 show that the ZSM-11 molecular sieve prepared by the present invention is used as a catalytic cracking catalyst, can improve coke selectivity, increase ethylene + propylene selectivity, has the characteristics of high low-carbon olefin selectivity and low coke generation, and has broad application prospects.
[0113] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a catalytic cracking catalyst, characterized in that: The following steps are involved: S1. Synthesize a ZSM-11 initial gel mixture according to a molar ratio of 0.12-0.2M2O: 0.005-0.01Al2O3: 1SiO2: 10-30H2O: 0.3-0.8(TBA)2O, and crystallize the gel mixture for 2-11 hours to obtain a pre-crystallization solution; wherein M is an alkali metal, Al2O3 is an aluminum source, SiO2 is a silicon source, and (TBA)2O is a template; S2, in the same proportion as the pre-crystallization solution, without adding a template, a silicon source, an aluminum source, an alkali source and water are prepared into a ZSM-11 initial gel solution; S3, adding the pre-crystallization solution in step S1 to the initial gel solution in step S2 to obtain a gel mixture, and further crystallizing to obtain a ZSM-11 molecular sieve crystallization solution; S4, separating, cooling, filtering and washing the ZSM-11 molecular sieve crystallization liquid, and modifying the obtained filter cake by ammonium salt exchange and roasting to obtain ZSM-11 molecular sieve; S5. Based on 100 parts of the dry basis of the catalyst, 15-40 parts of ZSM-11 molecular sieve, 5-15 parts of Y-type molecular sieve, 5-15 parts of a binder, 35-75 parts of clay and water are slurried, spray-formed, and calcined to obtain a catalytic cracking catalyst.
2. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step S1, the molar ratio of the components in the ZSM-11 initial gel mixture is 0.14-0.18M2O: 0.005-0.01Al2O3: 1SiO2: 15-25H2O: 0.4-0.7(TBA)2O; the molar ratio of Si atoms to Al atoms in the ZSM-11 initial gel mixture is 50-100.
3. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: The alkali metal is Na, K or Li; the silicon source is at least one of alkaline silica sol, silica gel and water glass; the aluminum source is at least one of aluminum chloride, aluminum sulfate and aluminum nitrate; and the template is a tetrabutylammonium template.
4. The method for preparing a catalytic cracking catalyst according to claim 3, characterized in that: The tetrabutylammonium template agent is at least one of tetrabutylammonium bromide and tetrabutylammonium hydroxide.
5. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step S1, the crystallization temperature is 150°C-170°C and the time is 2-4 hours; in step S3, the crystallization temperature is 150°C-170°C and the time is 24-72 hours.
6. The method for preparing a catalytic cracking catalyst according to claim 5, characterized in that: In step S3, the crystallization time is 48-60 hours.
7. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step S3, the amount of the pre-crystallization solution added is 10 wt% to 50 wt% of the initial gel solution.
8. The method for preparing a catalytic cracking catalyst according to claim 7, characterized in that: In step S3, the amount of the pre-crystallization solution added is 25 wt% to 50 wt% of the initial gel solution.
9. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step S4, the ammonium salt exchange modification of the ZSM-11 molecular sieve adopts: at least one of ammonium chloride, ammonium nitrate and ammonium sulfate is exchanged with the ZSM-11 molecular sieve and filtered 1-3 times until Na2O is less than 0.5wt%.
10. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step S5, ZSM-5 molecular sieve, metal modification element B, and phosphorus-containing substances are also added; based on 100 parts of the dry basis mass of the catalyst, 15-40 parts of ZSM-11 molecular sieve, 0-15 parts of ZSM-5 molecular sieve, 5-15 parts of Y-type molecular sieve, 5-15 parts of binder, 35-75 parts of clay, 0-3 parts of metal modification element B, and 0-10 parts of phosphorus-containing substances, where phosphorus is calculated as P2O5, are slurried with water, spray-formed, and calcined to obtain a catalytic cracking catalyst.
11. The method for preparing a catalytic cracking catalyst according to claim 10, characterized in that: In step S5, the catalyst is formulated as follows: based on 100 parts of the dry mass of the catalyst, it consists of 18-28 parts of ZSM-11 molecular sieve, 3-8 parts of ZSM-5 molecular sieve, 5-10 parts of Y-type molecular sieve, 7-15 parts of binder, 40-50 parts of clay, 1-2 parts of metal modification element B, and 4-8 parts of phosphorus-containing substances, wherein phosphorus is calculated as P2O5.
12. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step S5, the ZSM-11 molecular sieve may be at least one of the ZSM-11 molecular sieve obtained in step S4 and the modified ZSM-11 molecular sieve; the modification method of the modified ZSM-11 molecular sieve is: adjusting the concentration of the ZSM-11 molecular sieve slurry obtained in step S4 to a solid content of 80 to 400 g / L, adding 0.3% to 5% of the weight of the molecular sieve to modify the modified metal element A salt, and performing exchange modification, wherein the metal modified element A includes Ag, Zn, rare earth elements, at least one chloride or nitrate of the molecular sieve, the exchange temperature is 0-100° C., the exchange time is 0.1-1.5 hours, and then 0-5% of the weight of the molecular sieve by phosphorus-containing substance is added under stirring, the phosphorus is calculated as P2O5, and the phosphorus-containing substance includes at least one of phosphoric acid, ammonium phosphate, ammonium hydrogen phosphate and diammonium phosphate. The reaction temperature is 0-100° C., the reaction time is 0.1-1 hour, and the modified ZSM-11 molecular sieve is obtained by filtering, washing with water, and roasting, or without filtering, washing with water, and roasting.
13. The method for preparing a catalytic cracking catalyst according to claim 12, characterized in that: In the modification method of the modified ZSM-11 molecular sieve, 0.5% to 2.5% of the weight of the molecular sieve is added with a salt of the modified metal element A.
14. The method for preparing a catalytic cracking catalyst according to claim 12, characterized in that: In the modification method of the modified ZSM-11 molecular sieve, 1-3% of phosphorus-containing substances by weight of the molecular sieve are added under stirring, where phosphorus is calculated as P2O5.
15. The method for preparing a catalytic cracking catalyst according to claim 12, characterized in that: The phosphorus-containing substance is ammonium phosphate.
16. The method for preparing a catalytic cracking catalyst according to claim 10, characterized in that: In step S5, the ZSM-5 molecular sieve includes at least one of HZSM-5, Ag, Zn, Fe, rare earth, and P-modified ZSM-5 molecular sieves; the Y-type molecular sieve is at least one of USY, HY, REY, REHY, and REUSY; the binder is at least one of aluminum sol, acidified pseudo-boehmite, acidic silica sol, and phosphate aluminum sol; the clay is at least one of kaolin, halloysite, porous stone, diatomaceous earth, and vesicle stone; the metal modification element B is at least one of Ag, Zn, Fe, La, and Ce elements; and the phosphorus-containing substance is at least one of phosphoric acid, ammonium phosphate, ammonium hydrogen phosphate, and ammonium dihydrogen phosphate.
17. The method for preparing a catalytic cracking catalyst according to claim 16, characterized in that: In step S5, the Y-type molecular sieve is USY and REUSY.
18. The method for preparing a catalytic cracking catalyst according to claim 16, characterized in that: In step S5, the phosphorus-containing substance is phosphoric acid.
Citation Information
Patent Citations
Microwave synthesis process for ZSM-11 molecular sieve
CN101531376A
Fluid catalyst for preparing olefin and arene and application of fluid catalyst
CN106607075A
Synthesizing method of surface aluminum enriched type ZSM-23 molecular sieve
CN109516471A
Millimeter-scale microspheric molecular sieve and preparation method thereof
CN110655090A
Process of producing clean diesel oil and low carbon olefin with residual oil and heavy fraction oil
CN101045884A