A seawater resistant water blocking tape and its production process
A seawater-resistant water-blocking tape using a composite resin and semi-conductive glue addresses the absorption and production challenges of existing tapes, ensuring effective seawater protection with enhanced safety and cost-efficiency.
Patent Information
- Application Number
- CN202211375892.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-04
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-11-04
AI Technical Summary
Existing water-blocking tapes for optical cables suffer reduced water absorption rates in seawater due to the high osmotic pressure of seawater, and their production processes are costly and hazardous, requiring low-temperature, oxygen-free environments.
A seawater-resistant water-blocking tape production process using a salt-resistant water-absorbing resin composite of sodium polyacrylate, sodium alginate, calcium lignin sulfonate, diatomaceous earth, and xanthan gum, combined with a semi-conductive glue of polyvinyl alcohol, polyacrylate emulsion, furnace black, and fatty alcohol polyoxyethylene ether, which is safer and simpler, maintaining good water absorption and expansion in seawater.
The tape achieves high water absorption and expansion in seawater with improved safety and reduced production costs, ensuring effective protection for optical cables in marine environments.
Smart Images

Figure BDA0003926635920000041 
Figure BDA0003926635920000051 
Figure BDA0003926635920000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water-blocking tapes, and in particular to a seawater-resistant water-blocking tape and a production process thereof. Background Art
[0002] The water-blocking tape for optical cables plays a role in sealing, waterproofing, moisture-proofing and buffering protection for optical cables. The main body of the water-blocking tape is made of a composite of non-woven fabric and highly absorbent material, and has the function of swelling upon absorbing water. Highly absorbent materials have excellent water absorption and water retention functions. There are many types of highly absorbent resins commonly used, the main types are polyacrylates, polyvinyl alcohols, vinyl acetate copolymers, polyurethanes, polyethylene oxides, starch adhesive copolymers, etc. Highly absorbent resins have a large water absorption rate in pure water, but in seawater, due to the presence of a large amount of Na + , K + , Ca 2+ Mg 2+ , Sr + , Cl - 、SO4 2- Br - 、HCO3 - 、CO3 2- 、F - Plasma, the osmotic pressure of seawater is higher than that of pure water, which causes the water absorption rate of the super absorbent resin to be greatly reduced, and it cannot meet the requirements of the water-blocking tape for use in seawater.
[0003] In the patent with publication number CN110497635A, the applicant used sodium alginate to graft and crosslink with acrylic acid under the initiation of ammonium cerium nitrate to synthesize a water-absorbing resin with salt resistance and high water absorption, so that the water-absorbing resin can maintain a good liquid absorption rate in seawater. In the process of further research, the applicant found that due to the oxidizing property of ammonium cerium nitrate, the reaction conditions of crosslinking sodium alginate and acrylic acid with ammonium cerium nitrate as an initiator are relatively high, requiring a lower temperature and an oxygen-free environment, thereby increasing the production cost, and the use of ammonium cerium nitrate is somewhat dangerous.
[0004] In view of this, the present application specifically proposes this application to develop a low-cost, high-safety production process for seawater-resistant water-blocking tape, so that the water-blocking tape can maintain good water absorption in seawater. Summary of the invention
[0005] In order to improve the water absorption of the water-blocking tape in seawater, reduce production costs and improve safety, the present application provides a seawater-resistant water-blocking tape and a production process thereof.
[0006] In the first aspect, the present application provides a production process of seawater resistant water blocking tape, which is implemented by the following technical solution:
[0007] A production process of seawater resistant water blocking tape comprises the following steps:
[0008] S1, coating the lower surface of the upper semi-conductive non-woven fabric with semi-conductive glue;
[0009] S2, after impregnating the lower semi-conductive non-woven fabric with semi-conductive glue, sprinkle a salt-resistant water-absorbing resin composite on the lower semi-conductive non-woven fabric; the salt-resistant water-absorbing resin composite is prepared by mixing a water-absorbing resin, sodium polyacrylate, sodium alginate, calcium lignin sulfonate, diatomaceous earth and xanthan gum in a mass ratio of 5:1:(0.5-0.7):(0.3-0.5):(0.1-0.15):(0.2-0.3);
[0010] S3, compounding the side of the upper semi-conductive non-woven fabric coated with the semi-conductive glue with the lower semi-conductive non-woven fabric, and drying them by rollers to obtain a seawater resistant water-blocking tape.
[0011] By adopting the above technical solution, the salt-resistant water-absorbing resin composite composed of water-absorbing resin, sodium polyacrylate, sodium alginate, calcium lignin sulfonate, diatomaceous earth and xanthan gum has good water absorption performance and good expansion in seawater, which can meet the requirements of water-blocking tape used in seawater and has high elongation. This is because sodium polyacrylate is a linear, soluble polymer compound, and the carboxyl groups on the molecular chain of sodium polyacrylate stretch the twisted polymer chain due to electrostatic repulsion; sodium alginate is a chain-like polymer compound that can complex Ca in seawater. 2+ Mg 2+ Calcium lignin sulfonate has a branched and cross-linked molecular structure and ionizable charged hydrophilic groups such as sulfonic acid and carboxyl groups, and has excellent dispersibility, adhesion and chelation. Diatomaceous earth contains a small amount of Al2O3, Fe2O3, CaO, and MgO, and has the properties of being porous, water-absorbent and highly permeable. Xanthan gum has extremely strong hydrophilicity, and its viscosity is not affected by ions in seawater. Xanthan gum molecules can form super-bonded ribbon-shaped spiral copolymers. The combined action of sodium polyacrylate, sodium alginate, calcium lignin sulfonate, diatomaceous earth and xanthan gum can not only ensure that the water-absorbent resin will not fall off, but also improve the elongation of the water-blocking tape, and also improve the salt resistance and water absorption of the salt-resistant water-absorbent resin composite.
[0012] At the same time, the production process of the seawater-resistant water-blocking tape provided in the present application has high safety, does not require a low-temperature oxygen-free environment, has low requirements for reaction conditions, has a simple production process, stable technical performance, and strong practicality.
[0013] Preferably, the weight average molecular weight of the sodium polyacrylate is 15,000.
[0014] Sodium polyacrylate with a weight average molecular weight of 15,000 has excellent swelling performance when in contact with water and good dispersibility, which is beneficial to improving the salt resistance and water absorption of the salt-resistant water-absorbent resin composite.
[0015] Preferably, the weight average molecular weight of the calcium lignin sulfonate is 10,000-15,000.
[0016] Calcium lignin sulfonate with a weight average molecular weight of 10,000-15,000 has good surface activity, more ionizable charged hydrophilic groups, and a suitable content of charged groups, thereby improving the dispersibility of the salt-resistant water-absorbing resin composite, and further improving the salt resistance and water absorption of the salt-resistant water-absorbing resin composite.
[0017] Preferably, the salt-resistant water-absorbing resin composite is prepared by mixing water-absorbing resin, sodium polyacrylate, sodium alginate, calcium lignin sulfonate, diatomaceous earth and xanthan gum in a mass ratio of 5:1:0.7:0.5:0.1:0.2.
[0018] When the mass ratio of water-absorbing resin, sodium polyacrylate, sodium alginate, calcium lignin sulfonate, diatomaceous earth and xanthan gum is 5:1:0.7:0.5:0.1:0.2, the salt-resistant water-absorbing resin composite has a good water-blocking effect in seawater, and the water-blocking tape has a fast expansion speed and a high expansion height in seawater.
[0019] Preferably, the lower layer of semi-conductive non-woven fabric is sprinkled with a salt-resistant water-absorbing resin composite to form a seawater-resistant barrier layer with a thickness of 0.08-0.12 mm.
[0020] Preferably, the semi-conductive glue is prepared by mixing polyvinyl alcohol, polyacrylate emulsion, furnace black, fatty alcohol polyoxyethylene ether and water in a mass ratio of (0.2-0.3):1:(0.08-0.1):(0.02-0.03):3.
[0021] Polyvinyl alcohol has both hydrophilic and hydrophobic functional groups. It is a water-soluble environmentally friendly high molecular polymer with excellent film-forming, emulsifying and bonding properties. Polyvinyl alcohol and polyacrylate emulsion work together to have good adhesion to the semi-conductive non-woven fabric and salt-resistant water-absorbing resin composite, which can ensure that the water-absorbing resin will not fall off, thereby increasing the elongation of the water-blocking tape. Fatty alcohol polyoxyethylene ether has excellent adhesion, permeability and diffusion, which is conducive to improving the penetration of semi-conductive glue into the fibers of semi-conductive non-woven fabrics, thereby increasing the elongation of the water-blocking tape. In addition, furnace black has excellent conductivity and is relatively cheap, which is conducive to reducing the production cost of water-blocking tape.
[0022] Preferably, the polyvinyl alcohol is PVA-2099.
[0023] The alcoholysis degree of PVA-2099 is 99.0-100.0%, and the viscosity is 68.0-78.0 mPa.s, which corresponds to a higher elongation of the water-blocking tape, a faster swelling speed in seawater, a higher swelling height in seawater, and an excellent water-blocking effect.
[0024] Preferably, in step S1, the coating amount of the semi-conductive glue is 80-100 g / m 2 .
[0025] Preferably, in the step S2, the lower layer of semi-conductive non-woven fabric is immersed in the semi-conductive glue for 5-10 minutes.
[0026] In the second aspect, the present application provides a seawater resistant water blocking tape, which is implemented by the following technical solution:
[0027] A seawater resistant water-blocking tape is prepared by the above production process.
[0028] The seawater-resistant water-blocking tape provided in the present application has excellent electrical conductivity, is directly wound around a copper conductor, has good seawater corrosion resistance, and has good expansion properties in seawater, thereby providing good protection for the inner core of the conductor.
[0029] In summary, this application has the following beneficial effects:
[0030] 1. This application adopts a salt-resistant water-absorbing resin composite composed of water-absorbing resin, sodium polyacrylate, sodium alginate, calcium lignin sulfonate, diatomaceous earth and xanthan gum, which has good water absorption performance and good expansion in seawater, can meet the requirements of water-blocking tape for use in seawater, and has high elongation.
[0031] 2. The production process adopted in this application has high safety, low requirements on reaction conditions and simple production process.
[0032] 3. This application uses a semi-conductive glue composed of polyvinyl alcohol, polyacrylate emulsion, furnace black, fatty alcohol polyoxyethylene ether and water, which has good adhesion properties to the semi-conductive non-woven fabric and salt-resistant water-absorbing resin composite, and can ensure that the water-absorbing resin will not fall off, thereby improving the elongation of the water-blocking tape. DETAILED DESCRIPTION
[0033] The present application is further described in detail below with reference to the embodiments.
[0034] Preparation Example
[0035] Preparation Examples 1-9 provide a salt-resistant water-absorbing resin composite, and Preparation Example 1 is used as an example for description below.
[0036] The salt-resistant water-absorbing resin composite provided in Preparation Example 1 is prepared in the following steps:
[0037] 500 g of water-absorbing resin, 100 g of sodium polyacrylate, 50 g of sodium alginate, 30 g of calcium lignin sulfonate, 10 g of diatomaceous earth and 20 g of xanthan gum were mixed evenly to obtain a salt-resistant water-absorbing resin composite;
[0038] Among them, the model of water-absorbing resin is CA-100T, which was purchased from Dongying Qimai New Materials Co., Ltd.;
[0039] The weight average molecular weight of sodium polyacrylate is 8000;
[0040] Sodium alginate, particle size 100 mesh, industrial grade;
[0041] Calcium lignin sulfonate has a weight average molecular weight of 5000 and was purchased from Tianjin Yezi Chemical Technology Co., Ltd.;
[0042] Diatomaceous earth, particle size 325 mesh, industrial grade;
[0043] Xanthan gum, technical grade.
[0044] The only difference between Preparation Examples 2-5 and Preparation Example 1 is that the quality of the raw materials used in preparing the salt-resistant water-absorbing resin composite is different, as shown in Table 1.
[0045] Table 1 Mass of raw materials for preparation of salt-tolerant water-absorbing resin composites in Preparation Examples 1-5 / g
[0046]
[0047] Preparation Example 6 is different from Preparation Example 3 only in that the weight average molecular weight of sodium polyacrylate is 15,000.
[0048] Preparation Example 7 is different from Preparation Example 6 only in that the weight average molecular weight of calcium lignin sulfonate is 10,000.
[0049] Preparation Example 8 is different from Preparation Example 6 only in that the weight average molecular weight of calcium lignin sulfonate is 15,000.
[0050] Preparation Example 9 is different from Preparation Example 6 only in that the weight average molecular weight of calcium lignin sulfonate is 30,000.
[0051] Preparation Examples 10-14 provide a semi-conductive glue, and Preparation Example 10 is used as an example for description below.
[0052] The semi-conductive glue provided in Preparation Example 10 is prepared in the following steps:
[0053] 0.2 kg of polyvinyl alcohol, 1 kg of polyacrylate emulsion, 0.08 kg of furnace black, 0.02 kg of fatty alcohol polyoxyethylene ether AEO-9 and 3 kg of water were mixed evenly to obtain a semi-conductive glue;
[0054] Among them, the polyvinyl alcohol is PVA-2499;
[0055] The model of polyacrylate emulsion is YC-3, which was purchased from Qingdao Zhuonengda Construction Technology Co., Ltd.
[0056] Preparation Examples 11-12 are different from Preparation Example 10 only in that the quality of the raw materials for preparing the semi-conductive glue is different, as shown in Table 2 for details.
[0057] Table 2 Mass of raw materials for preparing semi-conductive glue in Preparation Examples 10-12 / kg
[0058]
[0059] Preparation Example 13 is different from Preparation Example 12 only in that the polyvinyl alcohol is PVA-2099.
[0060] Preparation Example 14 is different from Preparation Example 12 only in that the polyvinyl alcohol is PVA-1788.
[0061] Preparation Comparative Example
[0062] Comparative Examples 1-4 were prepared to provide a salt-resistant water-absorbing resin composite.
[0063] Comparative Example 1 was prepared, which was different from Preparation Example 1 only in that calcium lignin sulfonate was not added.
[0064] Comparative Example 2 was prepared, which was different from Preparation Example 1 only in that diatomaceous earth was not added.
[0065] Comparative Example 3 was prepared, which was different from Preparation Example 1 only in that no xanthan gum was added.
[0066] Comparative Example 4 was prepared, which was different from Preparation Example 1 only in that no sodium alginate was added.
[0067] Comparative Example 5 was prepared to provide a semi-conductive glue.
[0068] Comparative Example 5 was prepared, which was different from Preparation Example 10 only in that no fatty alcohol polyoxyethylene ether AEO-9 was added.
[0069] Example
[0070] Embodiments 1-17 provide a seawater resistant water blocking tape, which is described below using Embodiment 1 as an example.
[0071] The production process of the seawater-resistant water-blocking tape provided in Example 1 comprises the following steps:
[0072] S1. Coat the lower surface of the upper semi-conductive polyester fiber non-woven fabric with semi-conductive glue at a coating amount of 80g / m 2 ;
[0073] S2, immersing the lower layer of semi-conductive polyester fiber non-woven fabric in semi-conductive glue for 10 minutes, and then sprinkling a salt-resistant water-absorbing resin composite on the lower layer of semi-conductive polyester fiber non-woven fabric to form a seawater-resistant water-blocking layer with a thickness of 0.08 mm;
[0074] S3, compounding the side of the upper semi-conductive polyester fiber non-woven fabric coated with the semi-conductive glue with the lower semi-conductive polyester fiber non-woven fabric, passing through a roller, and drying at 150° C. to obtain a seawater resistant water-blocking tape;
[0075] Wherein, the semi-conductive glue is derived from Preparation Example 10;
[0076] The salt-resistant water-absorbing resin composite is derived from Preparation Example 1.
[0077] Example 2 is different from Example 1 in that: in step S1, the coating amount of the semi-conductive glue is 100 g / m 2 .
[0078] Embodiment 3 is different from Embodiment 2 in that: in step S2, the semi-conductive polyester fiber non-woven fabric is immersed in the semi-conductive glue for 5 minutes.
[0079] The difference between Examples 4-8 and Example 2 is that the sources of the semi-conductive glue are different, as shown in Table 3 for details.
[0080] Table 3 Source of semi-conductive glue in Examples 2, 4-8
[0081]
[0082] The difference between Examples 9-16 and Example 6 is that the sources of the salt-resistant water-absorbing resin composite are different, as shown in Table 4 for details.
[0083] Table 4 Sources of salt-tolerant water-absorbing resin composites of Examples 6, 9-16
[0084]
[0085] Example 17 is different from Example 14 in that a salt-resistant water-absorbing resin composite is sprinkled on the lower layer of semi-conductive polyester fiber non-woven fabric to form a seawater-resistant water-blocking layer with a thickness of 0.12 mm.
[0086] Comparative Example
[0087] Comparative Examples 1-4 are different from Example 1 only in that the sources of the salt-resistant water-absorbing resin composite are different, as shown in Table 5 for details.
[0088] Table 5 Source of comparative examples 1-4 salt-resistant water-absorbing resin composite
[0089]
[0090] Performance test: The seawater-resistant water-blocking tapes prepared in Examples 1-17 and Comparative Examples 1-4 of the present application were covered on the surface of the copper conductor, and the expansion speed, expansion height and elongation of the water-blocking tapes in seawater were tested using JB / T10259-2014 "Water-blocking tapes for cables and optical cables". The test results are shown in Table 6.
[0091] Table 6 Test results
[0092]
[0093]
[0094] The following describes the present application in detail with respect to the test data in Table 6.
[0095] From the test data of Example 1 and Comparative Examples 1-4, it can be seen that the salt-resistant water-absorbing resin composite composed of water-absorbing resin, sodium polyacrylate, sodium alginate, calcium lignin sulfonate, diatomaceous earth and xanthan gum has good water absorption performance and good expansion in seawater, which can meet the requirements for the use of water-blocking tape in seawater and ensure that the water-absorbing resin will not fall off, thereby improving the elongation of the water-blocking tape.
[0096] From the test data of Examples 2 and 8, it can be seen that compared with Example 2, no fatty alcohol polyoxyethylene ether AEO-9 is added to the semi-conductive glue in Example 8, and the elongation of the corresponding water-blocking tape in Example 8 is significantly lower than the elongation of the corresponding water-blocking tape in Example 2. This is because fatty alcohol polyoxyethylene ether has excellent adhesion, permeability, and diffusivity, which is beneficial to improving the penetration of the semi-conductive glue into the fibers of the semi-conductive non-woven fabric, thereby improving the elongation of the water-blocking tape.
[0097] From the test data of Examples 5, 6, and 7, it can be seen that Example 5 is PVA-2499, the alcoholysis degree of PVA-2499 is 98.0-100.0%, and the viscosity is 45.0-50.0 mPa.s, Example 6 is PVA-2099, the alcoholysis degree of PVA-2099 is 99.0-100.0%, and the viscosity is 68.0-78.0 mPa.s, and Example 7 is PVA-1788, the alcoholysis degree of PVA-1788 is 98.0-1 00.0%, viscosity is 46.0-56.0mPa.s, the elongation of the water-blocking tape corresponding to PVA-2099 is significantly higher than that of the water-blocking tape corresponding to PVA-2499 and PVA-1788, and the expansion speed of the water-blocking tape corresponding to PVA-2099 in seawater is faster and the expansion height in seawater is higher. The water-blocking effect of the water-blocking tape corresponding to PVA-2099 in seawater is better than that of the water-blocking effect of the water-blocking tape corresponding to PVA-2499 and PVA-1788 in seawater.
[0098] From the test data of Examples 10 and 13, it can be seen that the weight average molecular weight of sodium polyacrylate in Example 10 is 8000, and the weight average molecular weight of sodium polyacrylate in Example 13 is 15000. The elongation of the water-blocking tape corresponding to Example 13 is significantly higher than the elongation of the water-blocking tape corresponding to Example 10, and the expansion speed of the water-blocking tape corresponding to Example 13 in seawater is faster and the expansion height in seawater is higher.
[0099] From the test data of Examples 13-16, it can be seen that the weight average molecular weight of calcium lignin sulfonate in Example 13 is 5000, the weight average molecular weight of calcium lignin sulfonate in Example 14 is 10000, the weight average molecular weight of calcium lignin sulfonate in Example 15 is 15000, and the weight average molecular weight of calcium lignin sulfonate in Example 16 is 30000. The performance of the corresponding water blocking tapes of Examples 14 and 15 is better than that of the water blocking tapes of Examples 13 and 16. This is because the weight average molecular weight of the lignin sulfonate in Example 13 is relatively low, which reduces the surface activity of the lignin sulfonate; while the weight average molecular weight of the lignin sulfonate in Example 16 is relatively high, and the ionizable charged hydrophilic groups of the lignin sulfonate will be reduced accordingly, resulting in poor dispersion of the lignin sulfonate, and reducing the charged group content of the salt-resistant water-absorbing resin composite, thereby reducing the salt resistance of the water blocking tape.
[0100] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.
Claims
1. A production process for seawater resistant water-blocking tape, characterized in that: The steps include: S1, coating the lower surface of the upper semi-conductive non-woven fabric with semi-conductive glue; S2, after impregnating the lower semi-conductive non-woven fabric with semi-conductive glue, sprinkle a salt-resistant water-absorbing resin composite on the lower semi-conductive non-woven fabric; the salt-resistant water-absorbing resin composite is prepared by mixing a water-absorbing resin, sodium polyacrylate, sodium alginate, calcium lignin sulfonate, diatomaceous earth and xanthan gum in a mass ratio of 5:1: (0.5-0.7): (0.3-0.5): (0.1-0.15): (0.2-0.3); S3, compounding the side of the upper semi-conductive non-woven fabric coated with the semi-conductive glue with the lower semi-conductive non-woven fabric, and drying them by rollers to obtain a seawater resistant water-blocking tape; The semi-conductive glue is prepared by mixing polyvinyl alcohol, polyacrylate emulsion, furnace black, fatty alcohol polyoxyethylene ether and water in a mass ratio of (0.2-0.3):1:(0.08-0.1):(0.02-0.03):3, and the polyvinyl alcohol is PVA-2099.
2. The production process of a seawater resistant water-blocking tape according to claim 1, characterized in that: The weight average molecular weight of the sodium polyacrylate is 15,000.
3. The production process of a seawater resistant water-blocking tape according to claim 1, characterized in that: The weight average molecular weight of the calcium lignin sulfonate is 10,000-15,000.
4. The production process of a seawater resistant water-blocking tape according to claim 1, characterized in that: The salt-resistant water-absorbing resin composite is prepared by mixing water-absorbing resin, sodium polyacrylate, sodium alginate, calcium lignin sulfonate, diatomaceous earth and xanthan gum in a mass ratio of 5:1:0.7:0.5:0.1:0.
2.
5. The production process of a seawater resistant water-blocking tape according to claim 1, characterized in that: The lower semi-conductive non-woven fabric is sprinkled with a salt-resistant water-absorbing resin composite to form a seawater-resistant barrier layer with a thickness of 0.08-0.12 mm.
6. The production process of a seawater resistant water-blocking tape according to claim 1, characterized in that: In the step S1, the coating amount of the semi-conductive glue is 80-100 g / m 2 .
7. The production process of a seawater resistant water-blocking tape according to claim 1, characterized in that: In the step S2, the lower layer of semi-conductive non-woven fabric is immersed in the semi-conductive glue for 5-10 minutes.
8. A seawater-resistant water-blocking tape prepared by the production process according to any one of claims 1 to 7.