Halogen-free flame-retardant resin composition and preparation method thereof, and insulated wire
By using a combination of olefin resin, metal hydroxide and high melting point gallic acid compounds in halogen-free flame retardant resin, the problems of insufficient flame retardant and unstable processing of existing halogen-free flame retardant are solved, and high Halogen-free flame-retardant resin composition with flame retardant properties and insulated wires with good mechanical properties.
Patent Information
- Application Number
- CN202111325232.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-10
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-11-10
AI Technical Summary
The existing halogen-free flame retardants are prone to produce harmful gases due to insufficient flame retardancy and unstable processing. In particular, high-content EVA resin compositions are expensive and have low strength.
采用烯烃系树脂、金属氢氧化物和没食子酸类化合物的组合物,没食子酸类化合物的熔点为205℃以上,平均粒径为20μm以下,通过混合和混炼制备无卤阻燃树脂组合物,并用于绝缘导线的绝缘层。
It achieves high flame retardancy, good tensile strength and ductility, and is easy to produce and process, green and environmentally friendly, avoiding the generation of harmful gases.
Smart Images

Figure CN116102813B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a resin composition, in particular to a halogen-free flame-retardant resin composition and a preparation method thereof, and an insulated wire. Background Art
[0002] In general, olefin resins are widely used as electrical insulating materials due to their excellent electrical properties, mechanical properties, and processability. In particular, ethylene-unsaturated ester random copolymers such as EVA (ethylene-vinyl acetate copolymer) resins are widely used in wires, cables, and building materials because they have a good balance of tensile properties, low-temperature properties, scratch resistance, hardness, etc.
[0003] Such ethylene-unsaturated ester random copolymers need to be flame-retarded to achieve flame retardancy when used as coating materials and building materials for electric wires and communication lines. In addition, since the filling property of the filler of the ethylene-based polymer is good, flame retardants have been added to these resins to achieve flame retardancy. In the past, halogen-based flame retardants were used as flame retardants.
[0004] However, such complexes have the problem of generating harmful gases when burned. Therefore, in recent years, halogen-free flame retardants that are blended with metal hydroxide flame retardants such as magnesium hydroxide and aluminum hydroxide have been used.
[0005] However, the flame retardancy of existing halogen-free flame retardants is insufficient. As described in Patent Document 1, a special EVA resin composition with a high EVA content is also used, but there are problems such as high price and low strength of the special EVA resin composition with a high EVA content.
[0006] Prior art literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2008-138125 Summary of the invention
[0008] Technical Problems to be Solved by the Invention
[0009] The present invention has been made in view of the above-mentioned technical problems, and an object of the present invention is to provide a halogen-free flame-retardant resin composition having high flame retardancy and excellent mechanical properties such as tensile strength and elongation.
[0010] Means for solving technical problems
[0011] According to one aspect of the present invention, a halogen-free flame retardant resin composition is provided, characterized in that it comprises an olefin resin, a metal hydroxide and a gallic acid compound, wherein the gallic acid compound has a melting point of above 205° C. and an average particle size of below 20 μm.
[0012] In the halogen-free flame-retardant resin composition, the added amount of the metal hydroxide is 50 to 180 parts by mass, preferably 80 to 150 parts by mass, relative to 100 parts by mass of the olefin-based resin.
[0013] In the above-mentioned halogen-free flame-retardant resin composition, the olefin-based resin is selected from one or more of the group consisting of ethylene-vinyl acetate copolymer resin, polyethylene resin, polypropylene resin, ethylene-methyl acrylate copolymer resin, ethylene-ethyl acrylate copolymer resin, ethylene-acrylic acid copolymer resin, and ethylene-α-olefin copolymer resin.
[0014] In the above halogen-free flame-retardant resin composition, the gallic acid compound is gallic acid and its derivatives, preferably at least one selected from the group consisting of gallic acid monohydrate, gallic acid anhydrate and tannic acid.
[0015] The amount of the gallic acid compound added is 10 to 50 parts by mass, preferably 20 to 45 parts by mass, and more preferably 30 to 45 parts by mass, relative to 100 parts by mass of the olefin resin.
[0016] In the above-mentioned halogen-free flame-retardant resin composition, the metal hydroxide is at least one of magnesium hydroxide and aluminum hydroxide.
[0017] The halogen-free flame-retardant resin composition further comprises a lubricant; relative to 100 parts by mass of the olefin resin, the amount of the lubricant added is 0.1 to 5 parts by mass, preferably 0.1 to 2 parts by mass.
[0018] In the above-mentioned halogen-free flame-retardant resin composition, the olefin-based resin is ethylene-vinyl acetate copolymer resin.
[0019] In the above-mentioned halogen-free flame-retardant resin composition, the average particle size of the gallic acid compound is less than 10 μm.
[0020] According to another aspect of the present invention, there is provided a method for preparing a halogen-free flame retardant resin composition, which is characterized in that it comprises the following steps: (1) mixing an olefin resin, a metal hydroxide, a gallic acid compound and a lubricant to obtain a mixture; and (2) kneading the mixture at a temperature below 200° C. to obtain the halogen-free flame retardant resin composition.
[0021] In the preparation method of the halogen-free flame-retardant resin composition, the melting point of the gallic acid compound is above 205° C., and the average particle size is below 20 μm, preferably below 10 μm.
[0022] According to another aspect of the present invention, there is provided an insulated wire, characterized by comprising: a conductor; and an insulating layer covering the conductor and comprising the above-mentioned halogen-free flame-retardant resin composition.
[0023] Effects of the Invention
[0024] According to the present invention, a halogen-free flame retardant which is easy to produce and process can be obtained, which is green and environmentally friendly, has high flame retardancy, and has good mechanical properties such as tensile strength and elongation. The halogen-free flame retardant resin composition and insulated wire effectively solve the problems of unstable processing, unstable performance, and easy generation of harmful gases in the existing halogen-free flame retardant composition. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a picture showing the crystal state of coarse particles of gallic acid monohydrate observed by an optical microscope.
[0026] Figure 2 This is a picture of gallic acid monohydrate after pulverization observed through an optical microscope. DETAILED DESCRIPTION
[0027] The present inventors have conducted intensive research on the above technical problems and found that a halogen-free flame-retardant resin composition having excellent mechanical properties such as flame retardancy and ductility can be obtained by adding a micronized gallic acid compound (average particle size of 20 μm or less).
[0028] The resin composition of the present invention and its preparation method and application will be described in further detail below in conjunction with specific examples. It should be understood that the following examples are only for illustrative purposes and explanation of the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope of protection of the present invention.
[0029] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0030] Gallic acid compounds
[0031] Gallic acid compounds having a melting point of 205° C. or higher include gallic acid monohydrate (melting point 253° C.), gallic acid anhydrate (melting point 253° C.), and tannic acid (melting point 218° C.).
[0032] From the viewpoint of flame retardancy, gallic acid monohydrate is preferred.
[0033] Gallic acid compounds are crystalline substances, and their coarse particles are as follows Figure 1 The rod-shaped crystals are shown.
[0034] Here, the gallic acid compound is finely divided by pulverization or other methods and then added to the olefin resin.
[0035] The average particle size of the gallic acid compound after micronization is preferably 20 μm or less. If the gallic acid compound is larger than 20 μm, the mechanical properties will deteriorate.
[0036] More preferably, the average particle size of the gallic acid compound is 10 μm or less.
[0037] Metal hydroxide
[0038] As the metal hydroxide, for example, magnesium hydroxide, aluminum hydroxide, calcium hydroxide, etc. can be selected. Among them, magnesium hydroxide and aluminum hydroxide with good flame retardant effect are preferred. The addition amount of metal hydroxides such as magnesium hydroxide and aluminum hydroxide is preferably 50 to 180 parts by mass relative to 100 parts by mass of olefin resin. When the addition amount of the metal hydroxide is 50 parts by mass or less, the flame retardant effect is poor, and when the addition amount is 180 parts by mass or more, the mechanical properties may deteriorate.
[0039] Olefin resin
[0040] As olefin-based resins, for example, EVA (ethylene-vinyl acetate copolymer) resin, PE (polyethylene) resin, PP (polypropylene) resin, EMA (ethylene-methyl acrylate copolymer) resin, EEA (ethylene-ethyl acrylate copolymer) resin, EAA (ethylene-acrylic acid copolymer) resin, ethylene-α-olefin copolymer resin, etc. can be selected.
[0041] Among them, EVA resin is preferred because it excels in flexibility, mechanical properties, processability, economy, etc.
[0042] Lubricants
[0043] The lubricant used in the halogen-free flame retardant resin composition may be a stearic acid lubricant, a fatty amide lubricant or a silicone lubricant. The present invention preferably uses a stearic acid lubricant, such as stearic acid, methyl stearate, butyl stearate and the like.
[0044] Other additives
[0045] In addition to the above-mentioned components, the halogen-free flame retardant resin composition may also contain other additives as required, for example, processing aids, bridging agents, bridging aids, ultraviolet absorbers, antioxidants, copper damage inhibitors, fillers, compatibilizers, stabilizers, etc.
[0046] In addition, other flame retardants may be used as flame retardant aids. For example, melamine cyanurate, phosphate ester, ammonium polyphosphate, zinc borate, etc. may be selected as flame retardant aids.
[0047] Preparation of halogen-free flame retardant resin composition
[0048] Next, a method for preparing the halogen-free flame-retardant resin composition is described.
[0049] The halogen-free flame retardant resin composition of the present embodiment is prepared by mixing an olefin resin, a metal hydroxide, a gallic acid compound and a lubricant in a prescribed ratio, and then mixing. Among them, an existing mixing device can be used for mixing, for example, a kneader, a Banbury mixer, a mixer, a twin-shaft mixing extruder, an open roller, etc. can be used. The mixing temperature can be appropriately adjusted, preferably below 200°C. If the mixing temperature is above 200°C, the olefin resin will decompose, which may cause the mechanical properties of the resin composition to deteriorate.
[0050] Example
[0051] Hereinafter, the present invention will be further described based on detailed examples, but the present invention is not limited to these examples.
[0052] Material
[0053] In this example, the following materials were used.
[0054] EVA resin
[0055] As the EVA resin, Nipoflex 627 manufactured by Tosoh Corporation of Japan was used.
[0056] Magnesium hydroxide
[0057] As magnesium hydroxide, KISUMA 5A manufactured by Kyowa Chemical Industry Co., Ltd. was used.
[0058] Aluminum hydroxide
[0059] As aluminum hydroxide, BF013S manufactured by Nippon Light Metal Co., Ltd. was used.
[0060] Gallic acid monohydrate
[0061] As gallic acid monohydrate, gallic acid monohydrate (coarse particles, average particle size 76 μm) produced by Fuji Film Wako Pure Chemical Industries, Ltd. was used. Figure 1The morphology of the gallic acid monohydrate is shown in FIG. The average particle size is calculated by measuring the long sides and short sides of 50 coarse particles (100 points in total).
[0062] Lubricants
[0063] As a lubricant, "Stearic acid: Lunac S-50V" manufactured by Kao Corporation was used.
[0064] Grinding of Gallic Acid Monohydrate
[0065] Gallic acid monohydrate was pulverized using Nanojetmizer NJ-50-B manufactured by Aisin Nanotech Co., Ltd. (average particle size: 2.1 μm). Figure 2 The morphology of the pulverized gallic acid monohydrate is shown in FIG. 1. The average particle size is the average value calculated by measuring the diameters of 50 pulverized products.
[0066] Preparation of halogen-free flame retardant resin composition
[0067] The materials were mixed according to the ratios shown in Table 1 below to prepare the halogen-free flame-retardant resin compositions of Examples 1-2 and Comparative Examples 1-2.
[0068] Example 1
[0069] In Example 1, as shown in Table 1, 100 parts by mass of Nipoflex 627 was used as the EVA resin; 125 parts by mass of KISUMA 5A was used as the magnesium hydroxide; 25 parts by mass of a crushed product of gallic acid monohydrate was used; and 0.2 parts by mass of Lunac S50V was used as the lubricant. The above reagents were mixed and kneaded using a 60 ml mixer to prepare a halogen-free flame retardant resin composition.
[0070] Example 2
[0071] In Example 2, a halogen-free flame-retardant resin composition was prepared in the same manner as in Example 1 except that magnesium hydroxide was replaced with aluminum hydroxide (BF013S).
[0072] Example 3
[0073] In Example 3, a halogen-free flame-retardant resin composition was prepared in the same manner as in Example 1 except that 50 parts by mass of magnesium hydroxide and 15 parts by mass of a pulverized product of gallic acid monohydrate were used.
[0074] Example 4
[0075] In Example 4, a halogen-free flame-retardant resin composition was prepared in the same manner as in Example 1 except that 180 parts by mass of magnesium hydroxide and 10 parts by mass of a pulverized product of gallic acid monohydrate were used.
[0076] Example 5
[0077] In Example 5, a halogen-free flame-retardant resin composition was prepared in the same manner as in Example 1 except that 105 parts by mass of magnesium hydroxide and 35 parts by mass of a pulverized product of gallic acid monohydrate were used.
[0078] Comparative Example 1
[0079] In Comparative Example 1, as shown in Table 1, 100 parts by mass of Nipoflex 627 was used as EVA resin; 200 parts by mass of KISUMA 5A was used as magnesium hydroxide; and 0.2 parts by mass of Lunac S50V was used as a lubricant. The above reagents were mixed and kneaded using a 60 ml mixer to prepare a halogen-free flame retardant resin composition.
[0080] Comparative Example 2
[0081] In Comparative Example 2, as shown in Table 1, 100 parts by mass of Nipoflex 627 was used as EVA resin; 125 parts by mass of KISUMA5A was used as magnesium hydroxide; 25 parts by mass of coarse particles of gallic acid monohydrate was used; and 0.2 parts by mass of LunacS50V was used as a lubricant. The above reagents were mixed and kneaded using a 60 ml mixer to prepare a halogen-free flame retardant resin composition.
[0082] Preparation of test pieces
[0083] The test piece of the present embodiment is produced by press-molding the above-mentioned halogen-free flame-retardant resin composition into a desired shape, thereby producing a test piece for evaluation.
[0084] Evaluation Method
[0085] Flame retardant
[0086] UL94V combustion test
[0087] N=5 test pieces were prepared with a size of 127 mm×13 mm×2 mm in thickness.
[0088] The test method is implemented based on UL94V.
[0089] The evaluation was performed as described below, among which V-0 was the highest flame retardancy and was also the target flame retardancy of the resin composition.
[0090] V-0>V-1>V-2>Unqualified
[0091] Tensile strength
[0092] A No. 6 dumbbell-shaped test piece with N=5 was prepared.
[0093] The tensile strength was measured at a tensile speed of 200 mm / min by the method specified in JIS K 7161 2014. In the present example, a tensile strength of 5 MPa or more was evaluated as having sufficient tensile strength.
[0094] ·Elongation
[0095] A No. 6 dumbbell-shaped test piece with N=5 was prepared.
[0096] The tensile strength was measured at a tensile speed of 200 mm / min by the method specified in JIS K 7161 2014. In the present example, when the elongation was 50% or more, it was evaluated as having sufficient ductility.
[0097] Evaluation results
[0098] The evaluation results are shown in Table 1.
[0099] It can be seen from Table 1 that Examples 1 to 5 all have excellent flame retardancy, tensile strength, and elongation.
[0100] On the other hand, in Comparative Example 1, gallic acid monohydrate was not added, and 200 parts by weight of magnesium hydroxide was added in large amounts, but both the flame retardancy and the ductility did not reach the target.
[0101] In Comparative Example 2, 25 parts by mass of coarse particles of gallic acid monohydrate were added, but Figure 1 As shown, the target was not achieved due to the large particles and low ductility.
[0102] [Table 1]
[0103]
[0104] Unit of composition: mass parts
[0105] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A halogen-free flame retardant resin composition, characterized in that: It comprises an olefin resin, a metal hydroxide, a gallic acid compound and a stearic acid lubricant, wherein the gallic acid compound is gallic acid monohydrate, and the amount of the gallic acid compound added is 10 to 50 parts by mass relative to 100 parts by mass of the olefin resin; the amount of the lubricant added is 0.1 to 5 parts by mass relative to 100 parts by mass of the olefin resin; The gallic acid compound has a melting point of 205° C. or higher and an average particle size of 20 μm or less.
2. The halogen-free flame retardant resin composition according to claim 1, wherein The amount of the metal hydroxide added is 50 to 180 parts by mass relative to 100 parts by mass of the olefin-based resin.
3. The halogen-free flame retardant resin composition according to claim 1, wherein The olefin resin is one or more selected from the group consisting of ethylene-vinyl acetate copolymer resin, polyethylene resin, polypropylene resin, ethylene-methyl acrylate copolymer resin, ethylene-ethyl acrylate copolymer resin, ethylene-acrylic acid copolymer resin, and ethylene-α-olefin copolymer resin.
4. The halogen-free flame retardant resin composition according to any one of claims 1 to 3, wherein The metal hydroxide is at least one of magnesium hydroxide and aluminum hydroxide.
5. The halogen-free flame retardant resin composition according to any one of claims 1 to 3, wherein The average particle size of the gallic acid compound is less than 10 μm.
6. A method for preparing the halogen-free flame retardant resin composition according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) mixing an olefin resin, a metal hydroxide, a gallic acid compound and a stearic acid lubricant to obtain a mixture; and (2) kneading the mixture at a temperature below 200° C. to obtain the halogen-free flame retardant resin composition.
7. An insulated wire, characterized in that: have: Conductors; and The insulating layer is coated on the conductor and comprises the halogen-free flame retardant resin composition according to any one of claims 1 to 5.