A black talc-based composite air purifier and preparation method thereof
Through the etching, grafting and compounding of black talc powder, an efficient black talc-based composite air purifier was prepared, which solved the problems of high cost and low adsorption of activated carbon formaldehyde adsorbents, and achieved efficient adsorption of formaldehyde and recycling have enhanced the comprehensive utilization value of black talc.
Patent Information
- Application Number
- CN202211445597.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-18
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-11-18
AI Technical Summary
The existing activated carbon formaldehyde adsorbents have high cost and low adsorption, making it difficult to completely remove indoor formaldehyde pollution, affecting human health.
The black talc powder is processed through etching, grafting and compounding processes to prepare a black talc composite air purifier, which increases its surfactant and pore structure, and combines mordenite and binder to form an efficient adsorbent.
It realizes efficient adsorption and recycling of formaldehyde, reduces production costs, expands the application field of black talc, and provides an economical and practical air purification solution.
Smart Images

Figure BDA0003949524050000071 
Figure BDA0003949524050000081 
Figure BDA0003949524050000082
Abstract
Description
Technical Field
[0001] The invention belongs to the field of comprehensive utilization of non-metallic minerals, and specifically relates to a black talc-based composite air purifier and a preparation method thereof. Background Art
[0002] The main source of indoor pollution is formaldehyde. The national health standard stipulates that the indoor formaldehyde concentration should not exceed 0.08 mg / m 3 Especially in rooms after decoration, the formaldehyde concentration seriously exceeds the standard, which has a great impact on human health. At present, almost all commercial formaldehyde adsorbents are activated carbon bags, but the adsorption capacity of activated carbon bags is small and difficult to regenerate, which makes the formaldehyde removal incomplete and there is also the problem of high cost.
[0003] The color of black talc ore is black, its chemical composition is relatively pure, the particles are fine, it has a flaky structure, a high specific surface area, and does not contain harmful minerals such as asbestos. Moreover, its reserves are huge, the mining cost is low, and the price is cheap. It is widely used in industrial products such as ceramics, papermaking, and fillers. Nowadays, most of the products of black talc are low-end products such as fillers, and there is still a lot of room for development in other high-end technology fields. The properties of black talc can be reasonably utilized for modification to improve the performance of black talc in other aspects. This move not only conforms to my country's new industrialization path and sustainable development strategy, but also can broaden the application field of black talc and increase the economic benefits brought by the black talc industry. Summary of the invention
[0004] In view of the high development cost and low adsorption capacity of activated carbon formaldehyde adsorbents, the present invention provides a method for preparing a black talc-based composite air purifier. The air purifier is synthesized through etching, grafting, compounding and other steps, has a simple operation process, good adsorption effect on polar air pollutants such as formaldehyde, and high recovery efficiency.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention provides a black talc-based composite air purifier, which is prepared by the following method:
[0007] (1) Etching of black talc: black talc powder with an average particle size of 200 to 500 nm (preferably an average particle size of 300 to 400 nm) is immersed in an aqueous solution of an alkaline substance with a total concentration of 1 to 4 mol / L (preferably 2 mol / L), heated and stirred at 60 to 90° C. for 6 to 10 hours (preferably heated and stirred at 70° C. for 7 hours), and the resulting reaction solution A is subjected to post-treatment A to obtain etched black talc powder; the alkaline substance in the aqueous solution of the alkaline substance is one or a mixture of two or more of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, and ammonium hydroxide (ammonia water).
[0008] The purpose of etching is to etch away part of the silicon between the flaky layers of the black talc, so that the pore structure of the black talc is richer and the surface of the black talc is enriched with active functional groups.
[0009] (2) taking the etched black talc powder described in step (1) in an organic solvent, adding a grafting agent, carrying out a grafting reaction at 50-90° C. (preferably 70° C.) for 3-8 h (preferably 5 h), and subjecting the obtained reaction solution B to post-treatment B to obtain grafted black talc powder; the grafting agent is one or a mixture of two or more of N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane (KH792), γ-aminopropyltriethoxysilane (KH550), γ-glycidyloxypropyltrimethoxysilane (KH560), and γ-mercaptopropyltrimethoxysilane (KH590) (preferably N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane); the mass ratio of the grafting agent to the etched black talc powder is 1:1-3 (preferably 1:1);
[0010] The purpose of grafting is to graft the hydroxyl groups rich in the surface of black talc and graft active groups to increase its adsorption capacity for formaldehyde.
[0011] (3) The grafted black talc powder, mordenite powder with an average particle size of 200 to 500 nm (preferably an average particle size of 300 to 400 nm) and a binder described in step (2) are mixed and granulated to obtain the black talc-based composite air purifier; the mass ratio of the grafted black talc powder, mordenite and binder is 1:0.5 to 3:0.2 to 0.5 (preferably 1:1:0.33).
[0012] Furthermore, the volume of the aqueous solution of the alkaline substance in step (1) is 1 to 5 mL / g (2.5 mL / g) based on the mass of the black talc powder.
[0013] Furthermore, the post-treatment in step (1) is as follows: the reaction solution is cooled to room temperature, centrifuged (in one embodiment of the present invention, centrifuged at 5000 rpm / min for 5 min), the obtained precipitate is centrifuged and washed with deionized water until it becomes neutral, dried, and sieved (200 mesh) to obtain the etched black talc powder.
[0014] Furthermore, the organic solvent in step (2) is one or a mixture of two or more of toluene, ethanol, methanol, and acetone (preferably one or a mixture of two or more of methanol and toluene, most preferably toluene).
[0015] Preferably, the volume of the organic solvent in step (2) is 1-5 ml / g (3 ml / g) based on the mass of the etched black talc powder.
[0016] Furthermore, the post-treatment B in step (2) is as follows: cooling the reaction solution B, centrifuging, resuspending and washing the obtained precipitate with anhydrous ethanol three times, drying the obtained lower layer solid (60° C.), grinding and sieving (200 mesh), and obtaining the grafted black talc powder.
[0017] Furthermore, the binder in step (3) is one or a mixture of two or more of polyvinyl alcohol (PVA), sodium carbonate, and tetraethyl orthosilicate (preferably polyvinyl alcohol).
[0018] In one embodiment of the present invention, the rotation speed of the granulation in step (3) is 32 r / min, and spherical particles with a diameter of 2 to 3 mm are obtained. The rotation speed can be set as required in actual production.
[0019] The present invention provides a black talc powder with an average particle size of 200 to 500 nm (preferably an average particle size of 300 to 400 nm) in step (1) prepared as follows: black talc (Guangfeng District, Shangrao City, Jiangxi Province) is crushed, ground, and sieved (200 meshes) to obtain black talc powder, ethanol and deionized water are added to the black talc powder, and wet ball milling is performed in a ball mill. After taking out the sample, it is resuspended and washed with deionized water, and the lower layer of solid in the centrifuge tube is taken, dried, ground and sieved (200 meshes) to obtain ultrafine black talc powder, whose average particle size is 200 to 500 nm; the volume ratio of the ethanol to the deionized water is 0.5 to 2:1 (preferably 1:1); the total volume of the ethanol and the deionized water is based on completely immersing the black talc powder. Preferably, the volume of the ethanol is 0.6-1.6 mL / g based on the mass of the black talc powder. The speed of the wet ball milling is 700-800 r / min, and the time is 8-10 hours. The temperature of the drying is 60-120° C. (preferably 80-100° C.), and the time is 12-15 hours.
[0020] The present invention provides a method for preparing the mordenite powder with an average particle size of 200 to 500 nm (preferably an average particle size of 300 to 400 nm) in step (3): crushing, grinding and sieving (200 meshes) mordenite (Jinyun, Jiangsu) to obtain mordenite powder, adding ethanol and deionized water to the mordenite powder, wet-milling in a ball mill, taking out the sample, resuspending and washing it with deionized water, taking the lower layer of solid in the centrifuge tube, drying it, grinding and sieving (200 meshes), and obtaining ultrafine mordenite powder with an average particle size of 200 to 500 nm; the volume ratio of the ethanol to the deionized water is 0.5 to 2:1 (preferably 1:1); the total volume of the ethanol and the deionized water is based on completely immersing the black talc powder. Preferably, the volume of the ethanol is 0.6-1.6 mL / g based on the mass of the mordenite powder. The speed of the wet ball milling is 700-800 r / min, and the time is 8-10 hours. The temperature of the drying is 60-120° C. (preferably 80-100° C.), and the time is 12-15 hours.
[0021] The present invention also provides an application of the black talc-based composite air purifier in adsorbing formaldehyde.
[0022] Compared with the existing materials, the beneficial effects of the present invention are: ball milling the black talc effectively improves the specific surface area of the black talc, etching it, not only can make the surface rich in active groups, but also can further improve the specific surface area, enrich its pores, and then carry out grafting activation, not only retain the structure of the graphene layer, but also enrich the active groups on the surface, and finally compound the high adsorption capacity of the silky zeolite, so that the adsorption of formaldehyde is greatly increased. The preparation process is simple, the raw materials are cheap and easy to obtain, the production scale is easy to control, green and environmentally friendly, and no secondary pollution will be generated. The present invention provides a new direction for the field of black talc adsorbents, and at the same time provides an effective and economical way to improve the comprehensive utilization of black talc ore. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 FT-IR images of black talc before and after grafting in Example 1. DETAILED DESCRIPTION
[0024] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments. Without departing from the content and scope of the present invention, changes in implementation should be included in the technical scope of the present invention.
[0025] Formaldehyde testing method: Place the formaldehyde detector (kanfur JQ151) in a sealed glass container with a size of 30cm×30cm×30cm, and pass formaldehyde into the sealed room to ensure that the concentration of formaldehyde is 0.5mg / m 3Then put in 50g of adsorbent particles for adsorption, observe the reading of the formaldehyde detector after 5 hours, and calculate the formaldehyde adsorption rate. Set up a blank control.
[0026] Example 1
[0027] (1) The following conditions are used to prepare black talc powder: black talc from Guangfeng, Jiangxi Province is crushed, ground, and sieved (200 mesh) to obtain black talc powder; 80 ml of ethanol and 80 ml of deionized water are added to 100 g of the black talc powder, and the mixture is placed in a ball mill and wet-ground at a speed of 800 r / min for 10 h; the sample is taken out, resuspended and washed with deionized water, centrifuged three times, and the lower layer of solid in the centrifuge tube is taken, dried at 80° C. for 12 h, and ground and sieved (200 mesh) to obtain ultrafine black talc powder with an average particle size of 300 nm.
[0028] (2) Etching of black talc: 80 g of the ultrafine black talc powder described in step (1) was placed in a 2 mol / L 200 ml NaOH solution and heated in a 70° C. water bath with stirring for 7 h, cooled to room temperature, centrifuged at 5000 rpm / min for 5 min, resuspended and washed with deionized water until the supernatant was neutral, dried, ground and sieved (200 mesh), to obtain etched black talc powder;
[0029] (3) Preparation of grafted black talc: 80 g of the etched black talc in step (2) was placed in 240 ml of toluene, 80 g of KH792 was added, and the mixture was placed in a reactor and heated at 70° C. for 5 h. The mixture was cooled and centrifuged to remove the solid layer. Anhydrous ethanol was added to resuspend and wash the solid layer, and then centrifuged. The process was repeated three times. The solid layer was removed and dried at 60° C. The mixture was taken out and ground and sieved (200 mesh) to obtain the grafted black talc.
[0030] (4) Preparation of mortar-like Jinyun zeolite: Jinyun zeolite ore produced in Jinyun, Jiangsu Province was selected, crushed, and ball-milled in the manner of step (1) to obtain an average particle size of 300 nm.
[0031] (5) Black talc-based composite air purifier: 30g grafted black talc powder, 30g moring zeolite and 10g PVA were granulated in a disc granulator at a disc speed of 32r / min to obtain spherical particles with a diameter of 2-3mm. The moring zeolite was crushed from the zeolite mine.
[0032] (6) The formaldehyde removal rate of the obtained product is 97.8%.
[0033] Example 2
[0034] The other operations are the same as those in Example 1, except that the type of grafting agent in step (3) is different, and the other conditions are the same. The types of grafting agents used are listed in the table below.
[0035] name Formaldehyde adsorption rate (%) 80g KH550 96.0 80g KH560 91.2 80g KH590 93.5 80g triethanolamine 86.2 80g p-aminobenzenesulfonic acid 89.5 80g hexamethylenetetramine 81.3
[0036] Example 3
[0037] The other operations are the same as in Example 1, except that the type of binder in step (5) is different, and the other conditions are the same. The types of grafting agents used are listed in the table below.
[0038]
[0039]
[0040] Example 4
[0041] The other operations are the same as those in Example 1, except for the difference in the mass ratio of black talc to moringa zeolite in step (5), and the other conditions are the same. The types of grafting agents used are listed in the table below.
[0042]
[0043] Example 5
[0044] The other operations are the same as those in Example 1, except that the type of organic solvent in step (3) is different, and the other conditions are the same. The types of grafting agents used are listed in the table below.
[0045] name Formaldehyde adsorption rate (%) 240ml ethanol 87.1 240ml methanol 90.2 240ml acetone 86.4
[0046] Comparative Example 1
[0047] (1) The following conditions are used to prepare black talc powder: black talc from Guangfeng, Jiangxi Province is crushed, ground, and sieved (200 mesh) to obtain black talc powder; 80 ml of ethanol and 80 ml of deionized water are added to 100 g of the black talc powder, and the mixture is placed in a ball mill and wet-ground at a speed of 800 r / min for 10 h; the sample is taken out, resuspended and washed with deionized water, centrifuged three times, and the lower layer of solid in the centrifuge tube is taken, dried at 80° C. for 12 h, and ground and sieved (200 mesh) to obtain ultrafine black talc powder with an average particle size of 300 nm.
[0048] (2) Etching of black talc: 80 g of the ultrafine black talc powder described in step (1) was placed in a 2 mol / L 200 ml NaOH solution and heated in a 70° C. water bath with stirring for 7 h, cooled to room temperature, centrifuged at 5000 rpm / min for 5 min, resuspended and washed with deionized water until the supernatant was neutral, dried, ground and sieved (200 mesh), to obtain etched black talc powder;
[0049] (3) Preparation of grafted black talc: 80 g of the etched black talc in step (2) was placed in 240 ml of toluene, 80 g of KH792 was added, and the mixture was heated at 70° C. for 5 h in a reaction kettle. The mixture was cooled and centrifuged to remove the solid layer. Anhydrous ethanol was added to resuspend and wash the solid layer, and the mixture was centrifuged. The process was repeated three times. The solid layer was removed and dried at 60° C. The solid layer was taken out and ground and sieved (200 mesh) to obtain the grafted black talc.
[0050] (4) Black talc-based air purifier: 60 g of grafted black talc and 10 g of PVA were granulated in a granulator to obtain spherical particles with a diameter of 2 to 3 mm.
[0051] (5) The formaldehyde removal rate of the obtained product is 62%.
[0052] Comparative Example 2
[0053] (1) Moringa jinyunite: 60 g of moringa jinyunite and 10 g of PVA were granulated in a granulator to obtain spherical particles with a diameter of 2 to 3 mm.
[0054] (2) The formaldehyde removal rate of the obtained product is 40%.
[0055] Comparative Example 3
[0056] (1) The following conditions are used to prepare black talc powder: black talc from Guangfeng, Jiangxi Province is crushed, ground, and sieved (200 mesh) to obtain black talc powder; 80 ml of ethanol and 80 ml of deionized water are added to 100 g of the black talc powder, and the mixture is placed in a ball mill and wet-ground at a speed of 800 r / min for 10 h; the sample is taken out, resuspended and washed with deionized water, centrifuged three times, and the lower layer of solid in the centrifuge tube is taken, dried at 80° C. for 12 h, and ground and sieved (200 mesh) to obtain ultrafine black talc powder with an average particle size of 300 nm.
[0057] (2) Etching of black talc: 80 g of the ultrafine black talc powder described in step (1) was placed in a 2 mol / L 200 ml NaOH solution and heated in a 70° C. water bath with stirring for 7 h, cooled to room temperature, centrifuged at 5000 rpm / min for 5 min, resuspended and washed with deionized water until the supernatant was neutral, dried, ground and sieved (200 mesh), to obtain etched black talc powder;
[0058] (3) Preparation of mortar-like Jinyun zeolite: Select Jinyun zeolite ore produced in Jinyun, Jiangsu, crush it, and ball-mill it according to the method of step (1). Its particle size is the same as that of black talc.
[0059] (4) Black talc-based composite air purifier: 30g of black talc powder, 30g of moringen zeolite and 10g of PVA were granulated in a disc granulator at a disc speed of 32r / min to obtain spherical particles with a diameter of 2-3mm. The moringen zeolite was crushed from zeolite ore.
[0060] (5) The formaldehyde removal rate of the obtained product is 73.7%.
Claims
1. A black talc-based composite air purifier, characterized in that The black talc-based composite air purifier is prepared as follows: (1) Etching of black talc: taking black talc powder with an average particle size of 200 to 500 nm, immersing it in an aqueous solution of an alkaline substance with a total concentration of 1 to 4 mol / L, heating and stirring at 60 to 90° C. for 6 to 10 hours, and subjecting the obtained reaction solution A to post-treatment A to obtain etched black talc powder; the alkaline substance in the aqueous solution of the alkaline substance is one or a mixture of two or more of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, and ammonium hydroxide; (2) taking the etched black talc powder described in step (1) in an organic solvent, adding a grafting agent, carrying out a grafting reaction at 50-90° C. for 3-8 hours, and subjecting the obtained reaction solution B to post-treatment B to obtain grafted black talc powder; the grafting agent is one or a mixture of two or more of N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, and γ-mercaptopropyltrimethoxysilane; the mass ratio of the grafting agent to the etched black talc powder is 1:1-3; (3) The grafted black talcum powder, mordenite powder with an average particle size of 200 to 500 nm and a binder described in step (2) are mixed and granulated to obtain the black talc-based composite air purifier; the mass ratio of the grafted black talcum powder, mordenite and binder is 1:0.5 to 3:0.2 to 0.
5.
2. The black talc-based composite air purifier according to claim 1, characterized in that: The volume of the aqueous solution of the alkaline substance in step (1) is 1 to 5 mL / g based on the mass of the black talc powder.
3. The black talc-based composite air purifier according to claim 1, characterized in that: The post-treatment in step (1) is as follows: the reaction solution is cooled to room temperature, centrifuged, the obtained precipitate is centrifuged and washed with deionized water until it is neutral, dried, and sieved to obtain the etched black talc powder.
4. The black talc-based composite air purifier according to claim 1, characterized in that: The grafting agent described in step (2) is N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane.
5. The black talc-based composite air purifier according to claim 1, characterized in that: The organic solvent in step (2) is one or a mixture of two or more of toluene, ethanol, methanol and acetone.
6. The black talc-based composite air purifier according to claim 1, characterized in that: The organic solvent in step (2) is methanol, toluene or a mixture of both.
7. The black talc-based composite air purifier according to claim 1, characterized in that: The volume of the organic solvent in step (2) is 1-5 ml / g based on the mass of the etched black talc powder.
8. The black talc-based composite air purifier according to claim 1, characterized in that: The post-treatment B in step (2) is as follows: cooling the reaction solution B, centrifuging, resuspending and washing the obtained precipitate with anhydrous ethanol three times, drying the obtained lower layer solid, grinding and sieving, and obtaining the grafted black talc powder.
9. The black talc-based composite air purifier according to claim 1, characterized in that: The binder in step (3) is one or a mixture of two or more of polyvinyl alcohol, sodium carbonate, and tetraethyl orthosilicate.
10. Use of the black talc-based composite air purifier according to claim 1 in adsorbing formaldehyde.