A bio-based polymer and its preparation method and application

By modifying the ladder-shaped cross-linked structure of bio-based polymers and multi-site hydroxyl ring-opening reactions, the problem of insufficient performance of drilling fluids under high-temperature and high-salt conditions is solved, and efficient temperature and salt resistance and environmental protection are achieved, which is suitable for Drilling in deep wells.

CN116120903BInactive Publication Date: 2024-10-15CHINA WEST CONSTR GRP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310131499.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-11-24
Filing Date
2023-02-17
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing fluid loss additives in drilling fluids have poor performance under high temperature and high salt conditions, resulting in increased dosage, waste of resources and costs. In addition, traditional fluid loss additives have environmental pollution problems and are difficult to meet the needs of deep well drilling.

Method used

Bio-based raw materials with rigid structures and active groups are used, modified by anions of a highly stable electric double layer and specifically adsorbed cations, to prepare ladder-shaped cross-linked structure polymers to improve temperature and salt resistance, and through hydroxyl, The ring-opening reaction of amine groups and epoxy groups enhances structural stability, and the introduction of phosphate groups improves the adsorption capacity of suspended particles.

Benefits of technology

It significantly improves the degradation stability and salt resistance of drilling fluid under high-temperature and high-salt conditions, reduces high-temperature degradation and dehydration phenomena, complies with low-carbon environmental protection requirements, and has better performance than domestic and foreign products commercially available.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004084066020000121
    Figure BDA0004084066020000121
Patent Text Reader

Abstract

This application relates to the field of polymer synthesis technology, specifically disclosing a bio-based polymer, its preparation method, and its applications. The bio-based polymer comprises the following components in parts by weight: 20-30 parts of polyhydroxy biomass, 10-20 parts of polyol, 5-10 parts of allyl glycidyl ether, 5-10 parts of unsaturated carboxylic acid or anhydride, 2-5 parts of aminosulfonic acid, 5-10 parts of epichlorohydrin, 2-5 parts of secondary amine, 1-5 parts of sodium ethoxide, 1-3 parts of initiator, 8-15 parts of phosphorylation reagent, 0.5-1 part of inorganic suspending agent, and 10-20 parts of water. The bio-based polymer prepared by this invention exhibits excellent temperature and salt resistance, maintaining good filtration loss reduction performance even in saturated salt drilling fluids at temperatures reaching 220°C. Furthermore, the biomass raw materials used in the preparation method of this invention are renewable and biodegradable, complying with national low-carbon and environmental protection policies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of bio-based macromolecular material synthesis, and in particular relates to a bio-based polymer and a preparation method and application thereof. Background Art

[0002] Fluid loss reducers are one of the key materials for maintaining stable drilling fluid performance and safe and efficient drilling. In recent years, due to the rapid increase in energy demand, especially the consumption of oil and natural gas, the drilling of oil and gas wells has continued to deepen, and the number of deep wells and ultra-deep wells has increased accordingly. When the drilling of oil and gas wells reaches more than 4500m, the high temperature, high salt and high pressure formation environment makes the control of water loss and rheological properties of drilling fluids face huge challenges. Currently, commercially available fluid loss reducers are mainly used in shallow drilling, with a temperature resistance of no more than 180°C, and most of them contain environmentally harmful substances. Restricted by national environmental protection policies and laws and regulations, traditional fluid loss reducers will face elimination. Therefore, the temperature and salt resistance of drilling fluid fluid loss reducers and their low carbon and environmental protection have become the focus of attention of drilling fluid technicians and experts at home and abroad.

[0003] At present, the research on environmentally friendly drilling fluid loss reducers in China is mainly divided into two categories. One category is natural high molecular polymers, including starch, xanthan gum, cellulose, lignin, tannin, plant gum, etc., which are mainly used in upper shallow drilling and have a temperature resistance of about 120°C. The other category is high temperature resistant environmentally friendly drilling fluid loss reducers, which are mainly natural high molecular grafted polymers. Generally, functional monomers such as AM, AMPS, AA, NVP are grafted to synthesize multi-polymer high temperature resistant loss reducers with a temperature resistance of 180-200°C. Although there have been reports on environmentally friendly loss reducers with a temperature resistance of more than 180°C, their loss control under high temperature and high salt is still not ideal. In order to meet the drilling needs, the amount of loss reducer will be increased, which will cause a waste of resources and costs. Summary of the invention

[0004] In view of the shortcomings of existing drilling fluid filtration reducers in terms of temperature resistance and salt resistance and low-carbon and environmental protection, the present invention provides a bio-based polymer and a preparation method and application thereof. A bio-based raw material with a rigid structure and active groups is used as a precursor, and is modified by anions of a highly stable double electrical layer and cations with specific adsorption to clay to prepare a ladder-shaped cross-linked structure polymer, which can improve the temperature and salt resistance of the filtration reducer, provide technical support for deep well mining under extreme conditions of high temperature and high salt, and meet the national low-carbon and environmental protection strategic requirements.

[0005] To achieve the above purpose, the technical solution adopted by the present invention to solve the technical problem is:

[0006] A bio-based polymer, characterized in that it comprises the following components in parts by weight:

[0007] 20-30 parts of polyhydroxy biomass, 10-20 parts of polyols, 5-10 parts of allyl glycidyl ether, 5-10 parts of unsaturated carboxylic acid or anhydride, 2-5 parts of aminosulfonic acid, 5-10 parts of epichlorohydrin, 2-5 parts of secondary amine, 1-5 parts of sodium ethoxide, 1-3 parts of initiator, 8-15 parts of phosphorylation reagent, 0.5-1 part of inorganic suspending agent and 10-20 parts of water.

[0008] As a preferred embodiment, the polyhydroxy biomass is at least one of humic acid, fulvic acid, glucose, sodium gluconate, fructose, sucrose, lactose, soluble starch, cellulose ether and lignin sulfonate. Preferred polyhydroxy biomass is fulvic acid, sodium gluconate and lignin sulfonate. Among them, lignin sulfonate includes sodium salt, magnesium salt and calcium salt.

[0009] As a preferred embodiment, the polyol is at least one of polyethylene glycol, polypropylene glycol, ethylene glycol, and glycerol. As a solvent for biomass and a reactant with allyl glycidyl ether, the hydroxyl activity of the polyol should not be higher than the hydroxyl activity in the biomass to ensure the grafting rate of the biomass raw material. Preferred polyols are polyethylene glycol and glycerol.

[0010] As a preferred embodiment, the unsaturated carboxylic acid or anhydride is at least one of acrylic acid, methacrylic acid, itaconic acid, maleic acid and maleic anhydride. Preferred unsaturated carboxylic acids or anhydrides are methacrylic acid and maleic anhydride.

[0011] As a preferred embodiment, the secondary amine is at least one of dimethylamine, diethylamine, diethanolamine, and di-sec-butylamine. The CC main chain is bridged by the ring-opening reaction between the secondary amine and the epoxy group to prepare a ladder-shaped cross-linked structure, thereby improving the structural stability of the polymer and reducing the curling of the molecular conformation under high temperature and high salt conditions. Preferred secondary amines are dimethylamine and diethanolamine.

[0012] As a preferred embodiment, the initiator is hydrogen peroxide, vitamin C and ferrous sulfate, and the mass ratio of hydrogen peroxide, vitamin C and ferrous sulfate is 1: (0.2-0.5): (0.001-0.008). The preferred mass ratio of hydrogen peroxide, vitamin C and ferrous sulfate is 1: (0.3-0.4): (0.004-0.006)

[0013] As a preferred embodiment, the phosphorylation agent is at least one of polyphosphoric acid and phosphorus pentoxide. Introducing a phosphoric acid group into the molecular structure can enhance the adsorption of the fluid loss reducer on suspended particles, while enhancing the charge density, increasing the electrostatic repulsion, and improving the dispersion stability. The preferred phosphorylation agent is polyphosphoric acid.

[0014] As a preferred embodiment, the inorganic suspending agent is at least one of magnesium aluminum silicate, nano bentonite, nano montmorillonite, nano sepiolite, and fumed silica. The polymer molecules can be adsorbed onto the surface and interior of the inorganic suspending agent, which can improve the rheological properties such as viscosity of the fluid loss agent under high temperature and high salt conditions and enhance its rheological stability. The preferred inorganic suspending agents are magnesium aluminum silicate, nano montmorillonite, and fumed silica.

[0015] The present invention provides a method for preparing a bio-based polymer, which specifically comprises the following steps:

[0016] (1) The polyhydroxy biomass and the polyol are added to a reaction vessel from which air is excluded, the temperature is raised to 50° C., stirred to dissolve, and then the sodium ethoxide is added.

[0017] (2) raising the temperature to 60-70° C., continuously stirring, adding the allyl glycidyl ether within 1-2 hours, and keeping the temperature for reaction for 2-3 hours to obtain a biomass polyhydroxy-modified unsaturated ether.

[0018] (3) Add hydrogen peroxide as a base material to the biomass polyhydroxy-modified unsaturated ether obtained in step (2), dissolve the unsaturated carboxylic acid or anhydride in water as material A, dissolve the vitamin C and the ferrous sulfate in water as material B, control the reaction temperature between 40 and 50° C., add materials A and B simultaneously to the base material within 1 to 1.5 hours, and keep the temperature for reaction for 2 hours after the addition is completed to obtain a modified polymer A.

[0019] (4) Add the secondary amine and aminosulfonic acid to the modified polymer A obtained in step (3), then add the epichlorohydrin within 1 hour, control the reaction temperature not to exceed 70° C., and rapidly stir the reaction for 2 to 3 hours to obtain a cationic cross-linked polymer B.

[0020] (5) Adding the phosphorylation reagent in batches to the cationic cross-linked polymer B prepared in step (4), controlling the temperature not to exceed 85° C., to prepare a phosphorylated cross-linked polymer C.

[0021] (6) The inorganic suspending agent is mixed with water, and high-speed shear dispersion is performed at a rotation speed of 4000-6000 rpm for 0.5 h to obtain a suspension.

[0022] (7) Add the suspension prepared in step (6) to the phosphorylated cross-linked polymer C prepared in step 5), and continue stirring the reaction at a speed of 500 to 1000 rpm, while controlling the temperature at 40 to 60° C. for 1.5 to 3 hours to prepare a bio-based polymer.

[0023] The bio-based polymer can be applied to the fluid loss reducer of drilling fluid under high temperature and high salt conditions. The bio-based polymer has a cross-linked structure of CC and CO bonds with high energy, a stable double electric layer structure and specific adsorption groups, and has good temperature resistance and salt resistance. It can effectively solve the problems of high temperature degradation, high temperature and high salt molecular chain conformation, high temperature desorption, high temperature dehydration and high salt adsorption double electric layer stability of drilling fluid fluid loss reducer under high temperature and high salt conditions.

[0024] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0025] 1. The present invention adopts biomass with a large number of rigid structures and active groups as raw materials, which enhances the structural rigidity of the polymer. At the same time, the ring-opening reaction of multi-site hydroxyl groups plays a role of bridging side chains, forming a ladder-shaped cross-linked structure, further improving the structural stability under high temperature and high salt conditions, solving the problem of variable conformation of molecular chains under high temperature and high salt conditions, and improving the temperature and salt resistance of the polymer; and the biomass raw materials are renewable and biodegradable, which meets the national low-carbon and environmental protection policy requirements.

[0026] 2. The present invention utilizes the ring-opening reaction of hydroxyl, amine and epoxy groups to graft cationic segments with specific adsorption to clay onto polymer side chains, which can further reduce the problems of high-temperature desorption and high-temperature dehydration and improve the filtration loss reduction performance of the polymer.

[0027] 3. The present invention adopts high bond energy CC and CO bonds to construct the overall skeleton, avoiding the use of easily hydrolyzed groups such as ester bonds and amide bonds, reducing the high temperature degradation of the polymer and improving the high temperature resistance.

[0028] 4. The present invention introduces a highly stable double-layer anion structure into the structure through the ring-opening reaction of aminosulfonic acid and the sulfonic acid group of the biomass raw material, thereby improving the adsorption double layer stability of the polymer under high salt conditions and improving the salt resistance of the polymer.

[0029] 5. The present invention introduces a phosphate group into the molecular structure to enhance the adsorption of the fluid loss reducer on suspended particles, while enhancing the charge density, increasing the electrostatic repulsion, and improving the dispersion stability.

[0030] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. DETAILED DESCRIPTION

[0031] The present application is further described in detail below in conjunction with the embodiments, preparation examples and comparative examples. The raw materials involved in the present application can be obtained commercially. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the art without making creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] A method for preparing a bio-based polymer, the steps of which are as follows:

[0034] (1) 20 parts of humic acid and 10 parts of ethylene glycol were added to a reaction vessel purged of air, heated to 50°C, stirred to dissolve, and then 5 parts of sodium ethoxide were added.

[0035] (2) Raise the temperature to 60° C., continue stirring, add 5 parts of allyl glycidyl ether within 2 hours, and keep the temperature for reaction for 2 hours to obtain a biomass polyhydroxy-modified unsaturated ether.

[0036] (3) Add 2 parts of hydrogen peroxide as a base material to the biomass polyhydroxy-modified unsaturated ether of step 2), dissolve 10 parts of maleic acid in 2 parts of water as material A, and dissolve 0.8 parts of vitamin C and 0.004 parts of ferrous sulfate in 3 parts of water as material B. Control the reaction temperature at 40°C, add materials A and B simultaneously and mix with the base material within 1 hour, and keep the temperature for reaction for 2 hours after the addition is completed to obtain a bio-based modified polymer.

[0037] (4) Add 5 parts of di-sec-butylamine and 2 parts of aminosulfonic acid to the bio-based modified polymer of step 3), and then add 10 parts of epichlorohydrin within 1 hour, control the reaction temperature not to exceed 70°C, and rapidly stir the reaction for 2 hours to obtain a cationic cross-linked bio-based polymer.

[0038] (5) Add 8 parts of phosphorus pentoxide in batches to the cationic cross-linked bio-based polymer in step 4), and control the temperature not to exceed 85° C. to obtain a phosphorylated cross-linked bio-based polymer.

[0039] (6) 0.5 parts of nano-bentonite was mixed with 15 parts of water, and high-speed shear dispersion was performed at a rotation speed of 4000 rpm for 0.5 h to prepare a suspension.

[0040] (7) Add the suspension of step 6) to the phosphorylated cross-linked bio-based polymer of step 5), control the temperature at 40° C., and continue stirring the reaction at a speed of 500 rpm for 1.5 hours to obtain a bio-based polymer.

[0041] Example 2

[0042] A method for preparing a bio-based polymer, the steps of which are as follows:

[0043] (1) 15 parts of glucose, 15 parts of sodium gluconate and 20 parts of polypropylene glycol were added to a reaction vessel purged of air, heated to 50°C, stirred to dissolve, and then 3 parts of sodium ethoxide were added.

[0044] (2) Raise the temperature to 70° C., continue stirring, add 10 parts of allyl glycidyl ether within 2 hours, and keep the temperature for reaction for 3 hours to obtain a biomass polyhydroxy-modified unsaturated ether.

[0045] (3) Add 0.8 parts of hydrogen peroxide as a base material to the biomass polyhydroxy-modified unsaturated ether of step 2), dissolve 8 parts of acrylic acid in 1 part of water as material A, and dissolve 0.2 parts of vitamin C and 0.001 parts of ferrous sulfate in 3 parts of water as material B. Control the reaction temperature at 50°C, add materials A and B simultaneously and mix with the base material within 1.5 hours, and keep the temperature for reaction for 2 hours after the addition is completed to obtain a bio-based modified polymer.

[0046] (4) Add 2 parts of diethylamine and 5 parts of aminosulfonic acid to the bio-based modified polymer of step 3), and then add 5 parts of epichlorohydrin within 1 hour, control the reaction temperature not to exceed 70°C, and rapidly stir the reaction for 3 hours to obtain a cationic cross-linked bio-based polymer.

[0047] (5) Add 15 parts of phosphorus pentoxide in batches to the cationic cross-linked bio-based polymer in step 4), and control the temperature not to exceed 85° C. to obtain a phosphorylated cross-linked bio-based polymer.

[0048] (6) 1 part of fumed silica was mixed with 16 parts of water, and the mixture was dispersed by high-speed shearing at 6000 rpm for 0.5 h to prepare a suspension.

[0049] (7) Add the suspension of step 6) to the phosphorylated cross-linked bio-based polymer of step 5), control the temperature at 60° C. at a rotation speed of 1000 rpm, and continue stirring for 3 hours to obtain a bio-based polymer.

[0050] Example 3

[0051] A method for preparing a bio-based polymer, the steps of which are as follows:

[0052] (1) Add 10 parts of fructose, 10 parts of sucrose, 10 parts of lactose and 15 parts of glycerol into a reaction vessel purged of air, heat to 50°C, stir to dissolve, and then add 1 part of sodium ethoxide.

[0053] (2) Raise the temperature to 70° C., continue stirring, add 8 parts of allyl glycidyl ether within 1 hour, and keep the temperature for reaction for 3 hours to obtain biomass polyhydroxy-modified unsaturated ether.

[0054] (3) Add 2.5 parts of hydrogen peroxide as a base material to the biomass polyhydroxy-modified unsaturated ether of step 2), dissolve 10 parts of itaconic acid in 5 parts of water as material A, and dissolve 0.4 parts of vitamin C and 0.02 parts of ferrous sulfate in 5 parts of water as material B. Control the reaction temperature at 50°C, add materials A and B simultaneously and mix with the base material within 1 hour, and keep the temperature for reaction for 2 hours after the addition is completed to obtain a bio-based modified polymer.

[0055] (4) Add 3 parts of diethanolamine and 3 parts of aminosulfonic acid to the bio-based modified polymer of step 3), then add 10 parts of epichlorohydrin within 1 hour, control the reaction temperature not to exceed 70°C, and rapidly stir the reaction for 3 hours to obtain a cationic cross-linked bio-based polymer.

[0056] (5) Add 15 parts of polyphosphoric acid in batches to the cationic cross-linked bio-based polymer of step 4), and control the temperature not to exceed 85° C. to obtain a phosphorylated cross-linked bio-based polymer.

[0057] (6) 0.5 parts of nano-sepiolite was mixed with 9 parts of water, and high-speed shear dispersion was performed at a rotation speed of 5000 rpm for 0.5 h to prepare a suspension.

[0058] (7) Add the suspension of step 6) to the phosphorylated cross-linked bio-based polymer of step 5), control the temperature at 50° C. at a rotation speed of 800 rpm, and continue stirring for 2.5 hours to obtain a bio-based polymer.

[0059] Example 4

[0060] A method for preparing a bio-based polymer, the steps of which are as follows:

[0061] (1) 10 parts of sodium lignin sulfonate, 20 parts of calcium lignin sulfonate and 20 parts of glycerol were added to a reaction vessel purged of air, heated to 50° C., stirred to dissolve, and then 3 parts of sodium ethoxide were added.

[0062] (2) Raise the temperature to 70° C., continue stirring, add 10 parts of allyl glycidyl ether within 2 hours, and keep the temperature to react for 2.5 hours to obtain a biomass polyhydroxy-modified unsaturated ether.

[0063] (3) Add 2 parts of hydrogen peroxide as a base material to the biomass polyhydroxy-modified unsaturated ether of step 2), dissolve 10 parts of methacrylic acid in 2 parts of water as material A, and dissolve 0.5 parts of vitamin C and 0.012 parts of ferrous sulfate in 5 parts of water as material B. Control the reaction temperature at 50°C, add materials A and B simultaneously and mix with the base material within 1.5 hours, and keep the temperature for reaction for 2 hours after the addition is completed to obtain a bio-based modified polymer.

[0064] (4) Add 4 parts of dimethylamine and 3 parts of aminosulfonic acid to the bio-based modified polymer of step 3), and then add 10 parts of epichlorohydrin within 1 hour, control the reaction temperature not to exceed 70°C, and rapidly stir the reaction for 2.5 hours to obtain a cationic cross-linked bio-based polymer.

[0065] (5) Add 12 parts of polyphosphoric acid in batches to the cationic cross-linked bio-based polymer of step 4), and control the temperature not to exceed 85° C. to obtain a phosphorylated cross-linked bio-based polymer.

[0066] (6) 0.5 parts of magnesium aluminum silicate was mixed with 10 parts of water, and the mixture was dispersed at a high speed of 6000 rpm for 0.5 h to obtain a suspension.

[0067] (7) Add the suspension of step 6) to the phosphorylated cross-linked bio-based polymer of step 5), control the temperature at 50° C. at a rotation speed of 1000 rpm, and continue stirring for 2 hours to obtain a bio-based polymer.

[0068] Example 5

[0069] A method for preparing a bio-based polymer, the steps of which are as follows:

[0070] (1) 18 parts of soluble starch, 2 parts of cellulose ether and 20 parts of ethylene glycol were added to a reaction vessel purged of air, heated to 50° C., stirred to dissolve, and then 5 parts of sodium ethoxide were added.

[0071] (2) Raise the temperature to 70° C., continue stirring, add 10 parts of allyl glycidyl ether within 1.5 hours, and keep the temperature for reaction for 3 hours to obtain a biomass polyhydroxy-modified unsaturated ether.

[0072] (3) Add 2.4 parts of hydrogen peroxide as a base material to the biomass polyhydroxy-modified unsaturated ether of step 2), dissolve 5 parts of maleic anhydride in 9 parts of water as material A, and dissolve 0.4 parts of vitamin C and 0.019 parts of ferrous sulfate in 3 parts of water as material B. Control the reaction temperature at 50°C, add materials A and B simultaneously and mix with the base material within 1.5 hours, and keep the temperature for reaction for 2 hours after the addition is completed to obtain a bio-based modified polymer.

[0073] (4) Add 3 parts of diethylamine and 4 parts of aminosulfonic acid to the bio-based modified polymer of step 3), and then add 9 parts of epichlorohydrin within 1 hour, control the reaction temperature not to exceed 70°C, and rapidly stir the reaction for 3 hours to obtain a cationic cross-linked bio-based polymer.

[0074] (5) Add 10 parts of phosphorus pentoxide in batches to the cationic cross-linked bio-based polymer in step 4), and control the temperature not to exceed 85° C. to obtain a phosphorylated cross-linked bio-based polymer.

[0075] (6) 0.8 parts of nano-montmorillonite was mixed with 8 parts of water, and high-speed shear dispersion was performed at a rotation speed of 5500 rpm for 0.5 h to prepare a suspension.

[0076] (7) Add the suspension of step 6) to the phosphorylated cross-linked bio-based polymer of step 5), control the temperature at 55° C. at a rotation speed of 600 rpm, and continue stirring for 2 h to obtain a bio-based polymer.

[0077] Example 6

[0078] A method for preparing a bio-based polymer, the steps of which are as follows:

[0079] (1) Add 25 parts of fulvic acid and 15 parts of polyethylene glycol into a reaction vessel from which air is excluded, heat to 50°C, stir to dissolve, and then add 4 parts of sodium ethoxide.

[0080] (2) Raise the temperature to 65° C., continue stirring, add 9 parts of allyl glycidyl ether within 1.5 hours, and keep the temperature for reaction for 2.5 hours to obtain a biomass polyhydroxy-modified unsaturated ether.

[0081] (3) Add 1.5 parts of hydrogen peroxide as a base material to the biomass polyhydroxy-modified unsaturated ether of step 2), dissolve 6 parts of maleic anhydride in 9 parts of water as material A, and dissolve 0.5 parts of vitamin C and 0.075 parts of ferrous sulfate in 2 parts of water as material B. Control the reaction temperature at 45°C, add materials A and B simultaneously to the base material within 1.5 hours, and keep the temperature for reaction for 2 hours after the addition is completed to obtain a bio-based modified polymer.

[0082] (4) Add 3 parts of diethanolamine and 5 parts of aminosulfonic acid to the bio-based modified polymer of step 3), and then add 10 parts of epichlorohydrin within 1 hour, control the reaction temperature not to exceed 70°C, and rapidly stir the reaction for 3 hours to obtain a cationic cross-linked bio-based polymer.

[0083] (5) Add 12 parts of polyphosphoric acid in batches to the cationic cross-linked bio-based polymer of step 4), and control the temperature not to exceed 85° C. to obtain a phosphorylated cross-linked bio-based polymer.

[0084] (6) 0.5 parts of nano-montmorillonite was mixed with 9 parts of water, and high-speed shear dispersion was performed at a rotation speed of 5000 rpm for 0.5 h to prepare a suspension.

[0085] (7) Add the suspension of step 6) to the phosphorylated cross-linked bio-based polymer of step 5), control the temperature at 50° C. at a rotation speed of 800 rpm, and continue stirring for 2.5 hours to obtain a bio-based polymer.

[0086] Test example

[0087] The temperature and salt resistance of bio-based polymers were evaluated by comparing the filtration loss of 4wt% saturated salt-based drilling fluids mixed with 2wt% filtration reducer after aging at 200 and 220℃ for 16 hours.

[0088] Comparative Example 1 is a polymer prepared without adding polyhydroxy biomass, and other steps are consistent with Example 6.

[0089] Comparative Example 2 is a domestic drilling fluid loss reducer.

[0090] Comparative Example 3 is a foreign drilling fluid loss reducer. The blank group does not add a fluid loss reducer.

[0091] The test results of the comparative examples and embodiments are shown in Table 1.

[0092] Table 1 Filtration of 4wt% saturated salt-based drilling fluid mixed with 2wt% filtrate reducer and aged for 16 hours

[0093]

[0094] It can be seen from the data in the table that the experimental groups incorporating fluid loss reducers under high temperature and high salt conditions can effectively reduce the fluid loss of drilling fluid. Comparison of Examples 1 to 6 with Comparative Example 1 shows that the addition of polyhydroxy biomass raw materials during the synthesis of fluid loss agents can effectively improve the fluid loss reduction performance under high temperature and high salt conditions. Biomass raw materials have a large number of rigid structures and active groups, which enhance the structural rigidity of the polymer. At the same time, the ring-opening reaction of multi-site hydroxyl groups plays a role in bridging side chains, forming a ladder-shaped cross-linked structure, further improving the structural stability under high temperature and high salt conditions, and improving the temperature and salt resistance of the polymer.

[0095] Compared with Comparative Examples 2 and 3, the high-temperature and high-salt fluid loss reduction performance of the bio-based polymer of the present invention exceeds that of domestic commercial products, and reaches or even exceeds that of foreign commercial products, and has a good application effect.

[0096] In summary, the bio-based polymer of the present invention can meet the high requirements of high temperature resistance, salt resistance and environmental protection and degradability of the current drilling fluid loss reducer in deep well oil field exploitation.

[0097] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

[0098] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments may still be modified, or some or all of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A bio-based polymer, characterized in that The bio-based polymer comprises the following components in parts by weight: 20-30 parts of biomass, 10-20 parts of polyols, 5-10 parts of allyl glycidyl ether, 5-10 parts of unsaturated carboxylic acid or anhydride, 2-5 parts of aminosulfonic acid, 5-10 parts of epichlorohydrin, 2-5 parts of secondary amine, 1-5 parts of sodium ethoxide, 1-3 parts of initiator, 8-15 parts of phosphorylation reagent, 0.5-1 part of inorganic suspending agent, and 10-20 parts of water; The biomass is at least one of humic acid, fulvic acid, glucose, sodium gluconate, fructose, sucrose, lactose, soluble starch, cellulose ether and lignin sulfonate; The initiators are hydrogen peroxide, vitamin C and ferrous sulfate.

2. The bio-based polymer according to claim 1, characterized in that The polyol is at least one of polyethylene glycol, polypropylene glycol, ethylene glycol and glycerol.

3. The bio-based polymer according to claim 1, characterized in that The unsaturated carboxylic acid or anhydride is at least one of acrylic acid, methacrylic acid, itaconic acid, maleic acid and maleic anhydride.

4. The bio-based polymer according to claim 1, characterized in that The secondary amine is at least one of dimethylamine, diethylamine, diethanolamine and di-sec-butylamine.

5. The bio-based polymer according to claim 1, characterized in that The mass ratio of the hydrogen peroxide, vitamin C and ferrous sulfate is 1:(0.2-0.5):(0.001-0.008).

6. The bio-based polymer according to claim 1, characterized in that The phosphorylation agent is at least one of polyphosphoric acid and phosphorus pentoxide.

7. The bio-based polymer according to claim 1, characterized in that The inorganic suspending agent is at least one of magnesium aluminum silicate, nano bentonite, nano sepiolite and fumed silica.

8. The method for preparing a bio-based polymer according to claim 1, characterized in that: The following steps are involved: (1) adding the biomass and the polyol into a reaction vessel purged of air, heating to 50° C., stirring to dissolve, and then adding the sodium ethoxide; (2) raising the temperature to 60-70° C., continuously stirring, adding the allyl glycidyl ether within 1-2 hours, and keeping the temperature for reaction for 2-3 hours to obtain a biomass-modified unsaturated ether; (3) adding hydrogen peroxide as a base material to the biomass-modified unsaturated ether obtained in step (2), dissolving the unsaturated carboxylic acid or anhydride in water as material A, dissolving the vitamin C and the ferrous sulfate in water as material B, controlling the reaction temperature between 40 and 50° C., adding materials A and B simultaneously to the base material within 1 to 1.5 hours, and keeping the temperature for reaction for 2 hours after the addition is completed, to obtain a modified polymer A; (4) adding the secondary amine and aminosulfonic acid to the modified polymer A obtained in step (3), and then adding the epichlorohydrin within 1 hour, controlling the reaction temperature not to exceed 70° C., and rapidly stirring the reaction for 2 to 3 hours to obtain a cationic cross-linked polymer B; (5) adding the phosphorylation reagent to the cationic cross-linked polymer B obtained in step (4) in batches, controlling the temperature not to exceed 85° C., to obtain a phosphorylated cross-linked polymer C; (6) mixing the inorganic suspending agent with water, and dispersing the mixture at a speed of 4000 to 6000 rpm for 0.5 h to obtain a suspension; (7) Add the suspension prepared in step (6) to the phosphorylated cross-linked polymer C prepared in step 5), and continue stirring the reaction at a speed of 500 to 1000 rpm, while controlling the temperature at 40 to 60° C. for 1.5 to 3 hours to prepare a bio-based polymer.

9. Use of the bio-based polymer according to any one of claims 1 to 7 or the bio-based polymer prepared by the method for preparing the bio-based polymer according to claim 8, characterized in that: The bio-based polymer can be applied to a fluid loss reducer for drilling fluid under high temperature and high salt conditions.