A low-density Fe-Mn-Al-Ni-C steel plate and preparation method thereof
By adding nickel to the Fe-Mn-Al-C system and using a specific process, a low-density Fe-Mn-Al-Ni-C steel plate is prepared, which solves the technical lag problem in smelting and improves the strength and toughness of the steel plate. It meets the needs of lightweight vehicles and maintains good mechanical properties at high temperatures.
Patent Information
- Application Number
- CN202310044910.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-01-30
AI Technical Summary
The existing technology lacks detailed reports on the smelting of low-density high-strength steel, resulting in China's lagging industrialization process in this field. Moreover, the structure of traditional Fe-Mn-Al-C steel plates is unstable at high temperatures, affecting its strength and toughness.
Nickel is added to the traditional Fe-Mn-Al-C system, and a low-density Fe-Mn-Al-Ni-C steel plate is prepared through vacuum melting, large casting reduction, recrystallization, rolling, annealing and other processes. , ensuring its strength and toughness at room temperature and high temperature.
It improves the stability of the matrix structure of the steel plate, meets the demand for lightweight automobiles, and maintains good mechanical properties at 300 to 500°C, making it suitable for use in conventional vehicles and special vehicles.
Smart Images

Figure BDA0004054900940000061 
Figure BDA0004054900940000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of low-density steel and relates to a low-density Fe-Mn-Al-Ni-C steel plate and a preparation method thereof. Background Art
[0002] Research shows that there is a linear relationship between vehicle fuel consumption and vehicle weight. For every 10% reduction in vehicle weight, fuel consumption can be reduced by 6-8%. For every 1L reduction in fuel consumption, 2.45kg of CO2 will be reduced. 2 Therefore, lightweighting of automobiles can significantly alleviate the increasingly scarce energy situation and improve the increasingly deteriorating environmental conditions.
[0003] At present, there are two main ways to achieve lightweighting of automobiles: one is to use lightweight materials, such as aluminum, magnesium alloys, engineering plastics or carbon fiber composite materials; the other is to use thin-gauge high-strength steel to replace thick-gauge ordinary steel. Although lightweight materials such as aluminum alloys have good weight reduction potential, they have high production costs and difficult molding processes. Currently, they are only used in the manufacture of automobile transmissions, engines and other parts, as well as special vehicle bodies. At the same time, low-cost, high-performance high-strength steel has shown strong advantages and considerable weight reduction potential, which can meet the requirements of lightweight body.
[0004] Studies have shown that by adding a certain amount of aluminum to high-strength steel, under reasonable process control, automotive steel plates that combine low density and high strength properties can be obtained.
[0005] Aluminum-containing high-strength automotive steels include high-manganese Fe-(25~30)Mn-(2~4)Al-(2~4)Si system TWIP steel, Fe-(18~28)Mn-(9~12)Al-(0.7~1.2)C system SIP steel, and medium-manganese Fe-8Mn-5Al, Fe-11Mn-4Al-0.2C and other steels. Their room temperature structures are single-phase austenite or austenite-ferrite dual-phase structure, ensuring that the steel plates have high strength, toughness and formability.
[0006] Due to the excellent performance of high-strength steel plates, they will be used in automobiles in the future. Countries around the world are also actively conducting relevant research, and Pohang, South Korea, is a world leader in this regard. my country's research on low-density high-strength steel started relatively late, and there is only research on the process of "cast-steel plate", lacking detailed reports on smelting, and there is still a long way to go before industrialization. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a low-density Fe-Mn-Al-Ni-C steel plate and a preparation method thereof. Nickel is added to the traditional Fe-Mn-Al-C system in combination with a reasonable process design, thereby improving the matrix structure stability of the Fe-Mn-Al-C steel plate and ensuring the strength and toughness of the low-density material at room temperature and high temperature.
[0008] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0009] A low-density Fe-Mn-Al-Ni-C steel plate, whose chemical composition and mass percentage are: C: 1.2-1.5%, Mn: 18-20%, Al: 8-10%, Ni: 8-10%, Cr: 0.3-0.5%, S≤0.006%, P≤0.010%, and the balance is Fe and unavoidable impurity elements.
[0010] The steel plate is a single-phase austenite structure, the thickness of the steel plate is 2.5-5 mm, and the density is 6.8-7.0 g / cm 3 , strength-ductility product ≥55GPa·%
[0011] The method for preparing the above-mentioned low-density Fe-Mn-Al-Ni-C steel plate comprises the steps of vacuum melting, large reduction of ingot casting, recrystallization, rolling and annealing;
[0012] (1) Vacuum melting process: according to the target composition, the baked pure iron and electrolytic nickel plate are added into the crucible, the bottom is covered with electrolytic nickel, and the pure iron is placed on the top; the secondary silo is loaded with carbon powder, metal chromium, manganese aluminum iron, aluminum particles and other alloys, and the vacuum is evacuated, and the electric melting is started; after melting, the temperature is increased and refined for 30 to 50 minutes; then the vacuum is closed, argon gas is filled, and then carbon powder and metal chromium are added. After they are completely melted, manganese aluminum iron alloy is added until they are completely melted, and finally aluminum particles are added. After melting, they are stirred vigorously and cast into ingots;
[0013] (2) Ingot high pressure reduction process: the vacuum ingot is demoulded while hot, and the ingot is subjected to single-pass high pressure reduction rolling at 1180±20℃. After rolling, it is placed in a heating furnace and slowly cooled to room temperature;
[0014] (3) Recrystallization process: the billet after initial rolling is charged into a furnace and heated to 1130±10°C, and kept at this temperature for [(1-2)×bill thickness (mm)] min to obtain a billet with ASTM 4-5 grains;
[0015] (4) Rolling process: The billet is taken out of the furnace and rolled in multiple passes at 1080±20℃, and then water-cooled to room temperature;
[0016] (5) Annealing process: keep the steel plate at 400±10℃ for 10-15min, and finally take it out of the furnace and air cool it.
[0017] The vacuum smelting process comprises the following steps: adding the baked pure iron and electrolytic nickel plate into a crucible, laying the electrolytic nickel plate at the bottom and placing the pure iron on the top; loading the secondary silo with carbon powder, metallic chromium, manganese-aluminum-iron, aluminum particles and other alloys, evacuating the vacuum to below 5Pa, and starting electric smelting; after melting, heating to 1600-1620°C and refining for 30-50min; then closing the vacuum, filling with 30000-50000Pa argon gas, and then adding carbon powder and metallic chromium, and after completely melting, adding manganese-aluminum-iron alloy in batches until it is completely melted, and finally adding aluminum particles, stirring for 15-25min after melting, and casting into ingots.
[0018] The large reduction process of the casting billet has a single-pass reduction amount of 25 to 30%.
[0019] In the recrystallization process, the initial rolled billet is first heated to 680±10°C, kept warm for 1 to 2 hours, and then heated to 1130±10°C and kept warm.
[0020] The rolling process comprises 11 to 13 rolling passes, with a final rolling pass reducing the steel by 10 to 15% and the remaining single passes reducing the steel by 20 to 35%.
[0021] In the vacuum melting process, the mass proportions of manganese, aluminum and iron in the manganese-aluminum-iron alloy are 80%, 10% and 10% respectively.
[0022] The preparation process of the manganese-aluminum-iron alloy of the present invention is: firstly, pure iron is loaded into a vacuum induction furnace, vacuuming, and melting by electricity; the vacuum pump is stopped, argon gas is filled, aluminum and electrolytic manganese are added in sequence, and after melting, the manganese-aluminum-iron ingot is cast into an ingot; and the manganese-aluminum-iron ingot is cut into appropriate sizes at room temperature.
[0023] The beneficial effects of adopting the above technical solution are:
[0024] (1) The process flow of the present invention is simple and has a high component hit rate. In view of the difficulty in alloying aluminum and manganese, a process for alloying using manganese-aluminum-iron alloy blocks is provided. The density of manganese-aluminum-iron alloy blocks is much higher than that of aluminum, which can effectively solve the stratification problem of floating on the surface of molten steel after aluminum alloying in the traditional process; secondly, the addition of manganese-aluminum-iron alloy avoids the problem of manganese vapor volatilization caused by the high manganese vapor pressure after adding manganese alone, which can be said to kill two birds with one stone.
[0025] (2) Traditional Fe-Mn-Al ingots, due to the high content of aluminum, manganese, etc., the center of the ingot will produce serious segregation at the end of solidification, and will also become loose due to solidification shrinkage. The use of large reduction of the ingot can solve this problem. The present invention performs a single-pass large reduction rolling on the ingot at 1180±20℃, which can not only improve the degree of segregation at the end of solidification, but also compact the unsolidified end of the ingot center, effectively improving the quality of the ingot.
[0026] (3) Compared with the traditional low-density Fe-Mn-Al-C steel plate, the present invention adds 8-10% nickel, which makes the austenite structure more stable and improves the strength and toughness of the steel plate at room temperature. At the same time, the steel plate can maintain the structural stability at 300-500°C, which not only meets the use requirements of conventional vehicles, but also meets the use requirements of fire trucks, special vehicles and other vehicle body steel. DETAILED DESCRIPTION
[0027] The present invention is further described in detail below with reference to the embodiments.
[0028] Example 1
[0029] This embodiment uses a 500kg vacuum induction furnace, a Φ750×1100mm rolling mill, a 150kw heating furnace, and a 400×900×2000mm water cooling tank to produce low-density Fe-Mn-Al-Ni-C steel, and its chemical composition and target content are shown in Table 1. The production steps include:
[0030] 1) Vacuum furnace smelting
[0031] The bottom of the crucible is covered with 40kg of electrolytic nickel plates, and the upper part is placed with 300kg of pure iron rods; the secondary silo is loaded with 125kg of manganese-aluminum-iron alloy, 28kg of aluminum particles, 6kg of carbon powder, and 2.5kg of metallic chromium;
[0032] Evacuate to 5Pa, start power supply, and melt after 3 hours;
[0033] Adjust the vacuum degree to below 0.1Pa, raise the temperature to 1600℃, and refine for 40min;
[0034] Turn off the vacuum pump, fill with 40000Pa argon, add carbon powder and metal chromium, and turn off the power to cool down after melting; add manganese-aluminum-iron alloy in batches after film formation, turn on the stirring power, and add aluminum particles after all materials are melted;
[0035] After melting, take samples to test the composition and make fine adjustments. After the chemical composition is qualified, stir for 18 minutes;
[0036] The steel is tapped under electricity and cast into 250×400mm flat ingots.
[0037] 2) Large reduction of the casting
[0038] The casting was completed and the mold was removed 30 minutes later. The temperature of the ingot was monitored in real time. At 1200℃, the ingot was rolled in a single pass with a Φ750×1100mm rolling mill. The reduction was 75mm per pass and the specifications after rolling were 175×410mm. The ingot was then placed in a 150kw heating furnace for slow cooling.
[0039] 3) Recrystallization
[0040] The initial rolled billet was charged into a furnace, first heated to 680°C and kept at this temperature for 1.5 hours, then heated to 1130°C and kept at this temperature for 350 minutes to obtain ASTM 4 grade grains.
[0041] 4) Rolling
[0042] The billet is taken out of the furnace and rolled at 1060-1100℃. It is rolled to 3mm thickness through 11 passes. The process is 175mm→120mm→80mm→55mm→36mm→24mm→16mm→10.4mm→7mm→4.6mm→3.5mm→3mm. After rolling, the steel plate is placed in a water cooling tank and cooled to room temperature.
[0043] 5) Annealing
[0044] The heating furnace was heated to 400°C in advance, the steel plate was placed in it, kept warm for 15 minutes, and then air-cooled after being taken out of the furnace.
[0045] After the above-mentioned process, the composition and performance of the steel plate were tested. The chemical composition and actual content are shown in Table 1, and the performance test results are shown in Table 7.
[0046] Table 1: Chemical composition and content (wt%) of low-density Fe-Mn-Al-Ni-C steel of Example 1
[0047] element C Mn S P Cr Ni Al Target content 1.2 20 0.006 0.010 0.5 8 8 Actual content 1.21 19.8 0.006 0.010 0.48 8.01 8.12
[0048] Note: In Table 1, the balance is Fe and unavoidable impurity elements.
[0049] Example 2
[0050] This embodiment uses a 100kg vacuum induction furnace, a Φ750×1100mm rolling mill, a 150kw heating furnace, and a 400×900×2000mm water cooling tank to produce low-density Fe-Mn-Al-Ni-C steel, and its chemical composition and target content are shown in Table 2. The production steps include:
[0051] 1) Vacuum furnace smelting
[0052] A 10kg electrolytic nickel plate is placed at the bottom of the crucible, and a 58kg pure iron rod is placed on the top; 22.5kg manganese-aluminum-iron alloy, 7.5kg aluminum particles, 1.5kg carbon powder, and 0.3kg metallic chromium are loaded into the secondary silo;
[0053] Evacuate to 5Pa, start power supply, and melt after 2 hours;
[0054] Adjust the vacuum degree to below 0.1Pa, raise the temperature to 1620℃, and refine for 30min;
[0055] Turn off the vacuum pump, fill with 30000Pa argon, add carbon powder and metal chromium, and turn off the power to cool down after melting; add manganese-aluminum-iron alloy in batches after film formation, turn on the stirring power, and add aluminum particles after all materials are melted;
[0056] After melting, take samples to test the composition and make fine adjustments. After the chemical composition is qualified, stir for 15 minutes;
[0057] The steel is tapped under electricity and cast into 150×220mm flat ingots.
[0058] 2) Large reduction of the casting
[0059] The casting was completed and demoulding was carried out 30 minutes after the casting was completed. The temperature of the ingot was monitored in real time. At 1160℃, the ingot was rolled in a single pass with a Φ750×1100mm rolling mill. The single pass reduction was 37.5mm. The specifications after rolling were 112.5×230mm. It was then placed in a 150kw heating furnace for slow cooling.
[0060] 3) Recrystallization
[0061] The initial rolled billet was charged into a furnace, first heated to 690°C and kept at this temperature for 1 hour, then heated to 1140°C and kept at this temperature for 112.5 minutes to obtain ASTM 5 grade grains.
[0062] 4) Rolling
[0063] The billet is taken out of the furnace and rolled at 1060-1100℃. It is rolled to a thickness of 2.5mm through 11 passes. The process is 112.5mm→75mm→50mm→35mm→24mm→16mm→12mm→8mm→5.5mm→4mm→2.8mm→2.5mm. After rolling, the steel plate is placed in a water cooling tank and cooled to room temperature.
[0064] 5) Annealing
[0065] The heating furnace was heated to 410°C in advance, the steel plate was placed in it, kept warm for 10 minutes, and then air-cooled after being taken out of the furnace.
[0066] After the above-mentioned process, the composition and performance of the steel plate were tested. The chemical composition and actual content are shown in Table 2, and the performance test results are shown in Table 7.
[0067] Table 2: Chemical composition and content (wt%) of low-density Fe-Mn-Al-Ni-C steel of Example 2
[0068]
[0069]
[0070] Note: In Table 2, the balance is Fe and unavoidable impurity elements.
[0071] Example 3
[0072] This embodiment uses a 1000kg vacuum induction furnace, a Φ750×1100mm rolling mill, a 150kw heating furnace, and a 400×900×2000mm water cooling tank to produce low-density Fe-Mn-Al-Ni-C steel, and its chemical composition and target content are shown in Table 3. The production steps include:
[0073] 1) Vacuum furnace smelting
[0074] 90kg electrolytic nickel plate is laid on the bottom of the crucible, and 590kg pure iron rod is placed on the top; 237.5kg manganese-aluminum-iron alloy, 66.5kg aluminum particles, 14kg carbon powder, and 4kg metal chromium are loaded into the secondary silo;
[0075] Evacuate to 5Pa, start power supply, and melt after 4 hours;
[0076] Adjust the vacuum degree to below 0.1Pa, raise the temperature to 1620℃, and refine for 50min;
[0077] Turn off the vacuum pump, fill with 50000Pa argon, add carbon powder and metal chromium, and turn off the power to cool down after melting; add manganese-aluminum-iron alloy in batches after film formation, turn on the stirring power, and add aluminum particles after all materials are melted;
[0078] After melting, take samples to test the composition and make fine adjustments. After the chemical composition is qualified, stir for 20 minutes;
[0079] The steel is tapped under electricity and cast into 350×350mm square ingots.
[0080] 2) Large reduction of the casting
[0081] The casting was completed and demoulding was carried out 40 minutes after the casting was completed. The temperature of the ingot was monitored in real time. At 1200℃, the ingot was rolled in a single pass with a Φ750×1100mm rolling mill. The single pass reduction was 105mm. The specifications after rolling were 245×390mm. It was then placed in a 150kw heating furnace for slow cooling.
[0082] 3) Recrystallization
[0083] The initial rolled billet was charged into a furnace, first heated to 670°C and kept at this temperature for 2 hours, then heated to 1120°C and kept at this temperature for 490 minutes to obtain ASTM 4.5 grade grains.
[0084] 4) Rolling
[0085] The billet is taken out of the furnace and rolled at 1060-1100℃. It is rolled to 4mm thickness through 12 passes. The process is 245mm→190mm→125mm→85mm→60mm→40mm→26mm→18mm→12mm→8mm→5.5mm→4.4mm→4mm. After rolling, the steel plate is placed in a water cooling tank and cooled to room temperature.
[0086] 5) Annealing
[0087] The heating furnace was heated to 390°C in advance, the steel plate was placed in it, kept warm for 15 minutes, and then air-cooled after being taken out of the furnace.
[0088] After the above-mentioned process, the composition and performance of the steel plate were tested. The chemical composition and actual content are shown in Table 3, and the performance test results are shown in Table 7.
[0089] Table 3: Chemical composition and content (wt%) of low-density Fe-Mn-Al-Ni-C steel of Example 3
[0090] element C Mn S P Cr Ni Al Target content 1.4 19 0.006 0.010 0.4 9 9 Actual content 1.39 19.1 0.004 0.010 0.42 9.01 8.82
[0091] Note: In Table 3, the balance is Fe and unavoidable impurity elements.
[0092] Example 4
[0093] This embodiment uses a 3000kg vacuum induction furnace, a Φ750×1100mm rolling mill, a 150kw heating furnace, and a 400×900×2000mm water cooling tank to produce low-density Fe-Mn-Al-Ni-C steel, and its chemical composition and target content are shown in Table 4. The production steps include:
[0094] 1) Vacuum furnace smelting
[0095] 300kg of electrolytic nickel plate is laid on the bottom of the crucible, and 1740kg of pure iron rod is placed on the top; 675kg of manganese-aluminum-iron alloy, 232.5kg of aluminum particles, 39kg of carbon powder, and 15kg of metallic chromium are loaded into the secondary silo;
[0096] Evacuate to 5Pa, start power supply, and melt after 4 hours;
[0097] Adjust the vacuum degree to below 0.1Pa, raise the temperature to 1620℃, and refine for 50min;
[0098] Turn off the vacuum pump, fill with 50000Pa argon, add carbon powder and metal chromium, and turn off the power to cool down after melting; add manganese-aluminum-iron alloy in batches after film formation, turn on the stirring power, and add aluminum particles after all materials are melted;
[0099] After melting, take samples to test the composition and make fine adjustments. After the chemical composition is qualified, stir for 25 minutes;
[0100] The steel is tapped under electricity and cast into 400×600mm flat ingots.
[0101] 2) Large reduction of the casting
[0102] The casting was completed and demoulding was carried out 45 minutes after the casting was completed. The temperature of the ingot was monitored in real time. At 1200℃, the ingot was rolled in a single pass with a Φ750×1100mm rolling mill. The reduction amount of the single pass was 120mm. The specifications after rolling were 280×620mm. It was then placed in a 150kw heating furnace for slow cooling.
[0103] 3) Recrystallization
[0104] The initial rolled billet was charged into a furnace, first heated to 670°C and kept at this temperature for 2 hours, then heated to 1130°C and kept at this temperature for 560 minutes to obtain ASTM 4 grade grains.
[0105] 4) Rolling
[0106] The billet is taken out of the furnace and rolled at 1060-1100℃. It is rolled to 5mm thickness through 13 passes. The process is 280mm→220mm→176mm→140mm→112mm→85mm→60mm→40mm→28mm→20mm→13mm→8.5mm→5.8mm→5mm. After rolling, the steel plate is placed in a water cooling tank and cooled to room temperature.
[0107] 6) Annealing
[0108] The heating furnace was heated to 410°C in advance, the steel plate was placed in it, kept warm for 15 minutes, and then air-cooled after being taken out of the furnace.
[0109] After the above process, the composition and performance of the steel plate were tested. Its chemical composition and actual content are shown in Table 4, and the performance test results are shown in Table 7.
[0110] Table 4: Chemical composition and content (wt%) of low-density Fe-Mn-Al-Ni-C steel of Example 4
[0111] element C Mn S P Cr Ni Al Target content 1.3 18 0.006 0.010 0.5 10 10 Actual content 1.28 18.1 0.005 0.010 0.48 9.82 9.71
[0112] Note: In Table 4, the balance is Fe and unavoidable impurity elements.
[0113] Example 5
[0114] This embodiment uses a 500kg vacuum induction furnace, a Φ750×1100mm rolling mill, a 150kw heating furnace, and a 400×900×2000mm water cooling tank to produce low-density Fe-Mn-Al-Ni-C steel, and its chemical composition and target content are shown in Table 5. The production steps include:
[0115] 1) Vacuum furnace smelting
[0116] The bottom of the crucible is covered with 45kg of electrolytic nickel plates, and the upper part is placed with 295kg of pure iron rods; the secondary silo is loaded with 125kg of manganese-aluminum-iron alloy, 37.5kg of aluminum particles, 6kg of carbon powder, and 2.5kg of metallic chromium;
[0117] Evacuate to 5Pa, start power supply, and melt after 3 hours;
[0118] Adjust the vacuum degree to below 0.1Pa, raise the temperature to 1600℃, and refine for 40min;
[0119] Turn off the vacuum pump, fill with 45000Pa argon, add carbon powder and metal chromium, and turn off the power to cool down after melting; add manganese-aluminum-iron alloy in batches after film formation, turn on the stirring power, and add aluminum particles after all materials are melted;
[0120] After melting, take samples to test the composition and make fine adjustments. After the chemical composition is qualified, stir for 22 minutes;
[0121] The steel is tapped under electricity and cast into 250×400mm flat ingots.
[0122] 2) Large reduction of the casting
[0123] The casting was completed and demoulding was carried out 35 minutes after the casting was completed. The temperature of the ingot was monitored in real time. At 1170℃, the ingot was rolled in a single pass with a Φ750×1100mm rolling mill. The reduction in a single pass was 60mm. The specifications after rolling were 190×420mm. The ingot was then placed in a 150kw heating furnace for slow cooling.
[0124] 3) Recrystallization
[0125] The initial rolled billet was charged into a furnace, first heated to 690°C and kept warm for 1.5 hours, then heated to 1130°C and kept warm for 350 minutes to obtain ASTM 4 grade grains.
[0126] 4) Rolling
[0127] The billet is taken out of the furnace and rolled at 1060-1100℃. It is rolled to 3mm thickness through 12 passes. The process is 190mm→150mm→115mm→80mm→58mm→40mm→27mm→18mm→12mm→8mm→5.2mm→3.4mm→3mm. After rolling, the steel plate is placed in a water cooling tank and cooled to room temperature.
[0128] 5) Annealing
[0129] The heating furnace was heated to 405°C in advance, the steel plate was placed in it, kept warm for 10 minutes, and then air-cooled after being taken out of the furnace.
[0130] After the above-mentioned process, the composition and performance of the steel plate were tested. The chemical composition and actual content are shown in Table 5, and the performance test results are shown in Table 7.
[0131] Table 5: Chemical composition and content (wt%) of low-density Fe-Mn-Al-Ni-C steel of Example 5
[0132] element C Mn S P Cr Ni Al Target content 1.2 20 0.006 0.008 0.5 9 10 Actual content 1.21 19.89 0.005 0.006 0.49 9.06 9.93
[0133] Note: In Table 5, the balance is Fe and unavoidable impurity elements.
[0134] Example 6
[0135] This embodiment uses a 3000kg vacuum induction furnace, a Φ750×1100mm rolling mill, a 150kw heating furnace, and a 400×900×2000mm water cooling tank to produce low-density Fe-Mn-Al-Ni-C steel, and its chemical composition and target content are shown in Table 6. The production steps include:
[0136] 1) Vacuum furnace smelting
[0137] 300kg of electrolytic nickel plate is laid on the bottom of the crucible, and 1734.75kg of pure iron rod is placed on the top; 712.5kg of manganese-aluminum-iron alloy, 198.75kg of aluminum particles, 39kg of carbon powder, and 15kg of metallic chromium are loaded into the secondary silo;
[0138] Evacuate to 5Pa, start power supply, and melt after 3.5h;
[0139] Adjust the vacuum degree to below 0.1Pa, raise the temperature to 1600℃, and refine for 45min;
[0140] Turn off the vacuum pump, fill with 40000Pa argon, add carbon powder and metal chromium, and turn off the power to cool down after melting; add manganese-aluminum-iron alloy in batches after film formation, turn on the stirring power, and add aluminum particles after all materials are melted;
[0141] After melting, take samples to test the composition and make fine adjustments. After the chemical composition is qualified, stir for 20 minutes;
[0142] The steel is tapped under electricity and cast into 400×600mm flat ingots.
[0143] 2) Large reduction of the casting
[0144] The casting was completed and demoulding was carried out 40 minutes after the casting was completed. The temperature of the ingot was monitored in real time. At 1190℃, the ingot was rolled in a single pass with a Φ750×1100mm rolling mill. The reduction amount of the single pass was 110mm. The specifications after rolling were 290×615mm. It was then placed in a 150kw heating furnace for slow cooling.
[0145] 3) Recrystallization
[0146] The initial rolled billet was charged into a furnace, first heated to 680°C and kept at this temperature for 2 hours, then heated to 1130°C and kept at this temperature for 565 minutes to obtain ASTM 4 grade grains.
[0147] 4) Rolling
[0148] The billet is taken out of the furnace and rolled at 1060-1100℃. It is rolled to 5mm thickness through 13 passes. The process is 290mm→230mm→150mm→105mm→80mm→55mm→40mm→26mm→17mm→12mm→8mm→5.8mm→5mm. After rolling, the steel plate is placed in a water cooling tank and cooled to room temperature.
[0149] 5) Annealing
[0150] The heating furnace was heated to 400°C in advance, the steel plate was placed in it, kept warm for 10 minutes, and then air-cooled after being taken out of the furnace.
[0151] After the above-mentioned process, the composition and performance of the steel plate were tested. The chemical composition and actual content are shown in Table 6, and the performance test results are shown in Table 7.
[0152] Table 6: Chemical composition and content (wt%) of low-density Fe-Mn-Al-Ni-C steel of Example 6
[0153] element C Mn S P Cr Ni Al Target content 1.3 19 0.006 0.010 0.5 10 9 Actual content 1.28 18.9 0.005 0.007 0.48 9.82 8.92
[0154] Note: In Table 6, the balance is Fe and unavoidable impurity elements.
[0155] Table 7: Mechanical properties and density of steel plates in various examples
[0156]
[0157] The room temperature microstructure of the steel plates in the above embodiments is single-phase austenite, the strength-ductility product is ≥55GPa·%, and the density is ≤7.00g / cm 3 , is a low-density, high-strength and tough steel plate with excellent performance. Since the addition of Ni stabilizes the matrix phase structure at high temperature, the steel plate also has good mechanical properties at 300°C. From the comparison between Examples 1 and 2, it can be seen that when the addition amount of Ni is increased to 9.99%, the tensile strength of the steel plate at 300°C is higher, and the high-temperature performance is further improved, which fully meets the needs of new fire trucks, special vehicles and other body steel.
Claims
1. A method for preparing a low-density Fe-Mn-Al-Ni-C steel plate, characterized in that: The chemical composition and mass percentage of the steel plate are: C: 1.2-1.5%, Mn: 18-20%, Al: 8-10%, Ni: 8-10%, Cr: 0.3-0.5%, S≤0.006%, P≤0.010%, and the balance is Fe and unavoidable impurity elements; the preparation method includes vacuum melting, large reduction of ingot casting, recrystallization, rolling, and annealing processes; Vacuum smelting process: according to the target composition, the baked pure iron and electrolytic nickel plate are added into the crucible, the electrolytic nickel is laid on the bottom, and the pure iron is placed on the top; the secondary silo is loaded with carbon powder, metal chromium, manganese aluminum iron, and aluminum granule alloy, and vacuum is drawn, and electric smelting is started; after melting, the temperature is increased and refined for 30 to 50 minutes; then the vacuum is closed, argon gas is filled, and then carbon powder and metal chromium are added. After they are completely melted, manganese aluminum iron alloy is added until they are completely melted, and finally aluminum granules are added. After melting, they are stirred vigorously and cast into ingots; (2) Ingot high pressure reduction process: the vacuum ingot is demoulded while hot, and the ingot is subjected to single-pass high pressure reduction rolling at 1180±20℃. After rolling, it is placed in a heating furnace and slowly cooled to room temperature; (3) Recrystallization process: the billet after initial rolling is charged into a furnace and heated to 1130±10°C, and kept at this temperature for [(1-2)×bill thickness mm] min to obtain a billet with ASTM 4-5 grains; (4) Rolling process: The billet is taken out of the furnace and rolled for multiple passes at 1080±20℃, and then water-cooled to room temperature; (5) Annealing process: keep the steel plate at 400±10℃ for 10-15min, and finally take it out of the furnace and air cool it.
2. The method for preparing a low-density Fe-Mn-Al-Ni-C steel plate according to claim 1, characterized in that: The vacuum smelting process comprises the following steps: adding the baked pure iron and electrolytic nickel plate into a crucible, laying the electrolytic nickel plate at the bottom and placing the pure iron on the top; loading the secondary silo with carbon powder, metallic chromium, manganese-aluminum-iron and aluminum granule alloy, evacuating the vacuum to below 5Pa and starting electric smelting; after melting, heating to 1600-1620°C and refining for 30-50min; then closing the vacuum, filling with 30000-50000Pa argon gas, and then adding carbon powder and metallic chromium, and after completely melting, adding the manganese-aluminum-iron alloy in batches until it is completely melted, and finally adding aluminum granules, stirring for 15-25min after melting, and casting into ingots.
3. The method for preparing a low-density Fe-Mn-Al-Ni-C steel plate according to claim 2, characterized in that: The large reduction process of the casting billet has a single-pass reduction amount of 25 to 30%.
4. The method for preparing a low-density Fe-Mn-Al-Ni-C steel plate according to claim 3, characterized in that: In the recrystallization process, the initial rolled billet is first heated to 680±10°C, kept warm for 1 to 2 hours, and then heated to 1130±10°C and kept warm.
5. The method for preparing a low-density Fe-Mn-Al-Ni-C steel plate according to claim 4, characterized in that: The rolling process is performed for 11 to 13 passes, with a reduction of 10 to 15% in the final pass and a reduction of 20 to 35% in the remaining passes.
6. The method for preparing a low-density Fe-Mn-Al-Ni-C steel plate according to any one of claims 2 to 5, characterized in that: In the vacuum melting process, the mass proportions of manganese, aluminum and iron in the manganese-aluminum-iron alloy are 80%, 10% and 10% respectively.
7. The method for preparing a low-density Fe-Mn-Al-Ni-C steel plate according to claim 1, characterized in that: The steel plate is a single-phase austenite structure, the thickness of the steel plate is 2.5-5 mm, and the density is 6.8-7.0 g / cm 3 , strength-plasticity product ≥55GPa·%.
Citation Information
Patent Citations
Low-density high-plasticity NiAl-reinforced ultrahigh-strength steel and preparation method thereof
CN104711494A