A method and device for rapidly preparing carbon nanotube catalyst

By loading active metals in the form of spraying or spraying and passing them into alkaline gas to precipitate and aging, the preparation process of carbon nanotube catalysts is simplified, and the problems of wastewater generation and energy consumption caused by solid-liquid separation steps in the prior art are solved, and the problem of high wastewater generation and energy consumption is achieved. The preparation cycle is shortened and the production efficiency is improved to obtain carbon nanotube catalysts suitable for industrial production.

CN116135307BActive Publication Date: 2024-12-03SHANDONG DAZHAN NANO MATERIALS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111355934.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-16
Publication Date
2024-12-03
Estimated Expiration
2041-11-16

AI Technical Summary

Technical Problem

In the existing carbon nanotube catalyst preparation process, there are problems such as solid-liquid separation steps that lead to wastewater production, large energy consumption, long preparation cycle and poor morphology control, which is difficult to meet the needs of large-scale industrial production.

Method used

The active metal is loaded by spraying or spraying, and alkaline gas is introduced for precipitation and aging, avoiding solid-liquid separation operations, simplifying the drying steps, shortening the preparation cycle, and obtaining carbon nanotube catalysts through calcination, screening and reduction.

Benefits of technology

It has achieved shortening of the preparation cycle, improving production efficiency, and good control of the morphology of carbon nanotubes, and obtained a carbon nanotube catalyst with high load uniformity, large specific surface area and good conductivity, which is suitable for industrial mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116135307B_ABST
    Figure CN116135307B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a carbon nanotube catalyst, the method comprising providing a catalyst carrier and an active metal salt solution; infiltrating and mixing the active metal salt solution with the catalyst carrier; introducing alkaline gas into the obtained mixture to deposit and age the active metal to prepare a catalyst precursor; calcining, screening and reducing the catalyst precursor to prepare a carbon nanotube catalyst. The present invention also discloses an apparatus for preparing a carbon nanotube catalyst, a carbon nanotube catalyst prepared according to the method, and a carbon nanotube prepared using the carbon nanotube catalyst. The method for preparing a carbon nanotube catalyst of the present invention avoids solid-liquid separation operation, and has the characteristics of short preparation cycle and high production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method and device for preparing a carbon nanotube catalyst. The method for preparing a carbon nanotube catalyst of the present invention avoids solid-liquid separation operation and has the characteristics of short preparation cycle and high production efficiency. Background Art

[0002] As a one-dimensional nanomaterial, carbon nanotubes have excellent physical and mechanical properties. They are mainly coaxial circular tubes composed of several to dozens of layers of carbon atoms arranged in a hexagonal pattern. They have a very large aspect ratio, with a diameter usually between 1-100nm and a length between several microns and tens of centimeters. It is precisely because of its large aspect ratio that carbon nanotubes have excellent mechanical, electrical, electrical and thermal conductivity. Due to its excellent performance, carbon nanotubes have broad and potential application prospects in many fields such as catalyst carriers, rubber and plastic composites, electrochemical materials, and photoelectric sensors.

[0003] In the current carbon nanotube preparation process, except for some DC arc methods that do not require catalysts, other methods all require the participation of catalysts. The commercial preparation methods of carbon nanotube catalysts are mainly concentrated in the co-precipitation method and the gel method. Among them, the co-precipitation method requires the precipitation agent solution and the active metal solution to be added dropwise at a uniform rate. In addition to the need for solid-liquid separation in the process, a large amount of wastewater is generated at the same time; the gel method preparation of catalysts requires a large amount of solvent to be evaporated, which consumes a lot of energy, has a long preparation cycle, and has low production capacity release. In addition, there is a common problem that the morphology of the carbon nanotubes prepared in the end is not well controlled.

[0004] Therefore, the prior art still needs to develop a method for preparing carbon nanotube catalysts with a simple process and a device for the method, which does not require a solid-liquid separation step to generate wastewater, and the carbon nanotube catalyst prepared by the method can prepare carbon nanotubes with good morphology. Summary of the invention

[0005] The purpose of the present invention is to provide a method and device for preparing a carbon nanotube catalyst. The method has simple process, low cost and is easy to operate. The carbon nanotube catalyst prepared by the method can control the morphology of the finally prepared carbon nanotubes and is suitable for industrial large-scale production.

[0006] The present invention adopts the spraying or atomizing form to load the active metal and introduces alkaline gas for precipitation aging, which greatly simplifies the production and preparation process, avoids the solid-liquid separation operation, simplifies the drying operation, shortens the preparation cycle, eliminates the generation of sewage, and significantly improves the production efficiency. The reaction form of the gas makes the precipitation deposition more uniform and sufficient, and the size of the active site is smaller and finer, which can realize the batch continuous and stable preparation of carbon nanotube catalysts. The inventors have completed the present invention based on the above findings. The catalyst preparation process of the present invention is simple and stable, and the process conditions are easy to control, which can realize batch preparation. The catalyst loading rate prepared by the present invention is highly uniform, and the data such as specific surface area are stable. The carbon nanotubes prepared by chemical vapor deposition using the carbon nanotube catalyst obtained by the present invention have the characteristics of thin tube diameter and narrow distribution, good conductivity, and large specific surface area.

[0007] Therefore, one aspect of the present invention provides a method for preparing a carbon nanotube catalyst, the method comprising:

[0008] 1) Providing a catalyst carrier and an active metal salt solution;

[0009] 2) infiltrating and mixing the active metal salt solution with the catalyst support;

[0010] 3) introducing alkaline gas into the mixture obtained in step 2) to deposit and age the active metal to prepare a catalyst precursor;

[0011] 4) calcining, screening and reducing the catalyst precursor to prepare a carbon nanotube catalyst.

[0012] In one embodiment of the present invention, the infiltration mixing is performed in the form of spraying or atomizing.

[0013] In one embodiment of the present invention, in the infiltration and mixing step, the mixing mass ratio of the catalyst support to the active metal salt solution is 1:0.1-20.

[0014] In one embodiment of the present invention, the active metal salt solution comprises one or more metals selected from iron, cobalt, nickel, manganese, vanadium, zinc, copper, molybdenum, magnesium, aluminum, tungsten, calcium, chromium, and lanthanum.

[0015] In one embodiment of the present invention, the metal salt is one or a combination of nitrate, acetate, sulfate, chloride.

[0016] In one embodiment of the present invention, the concentration of the active metal salt solution is 0.05-10 mol / L.

[0017] In one embodiment of the present invention, the alkaline gas is selected from ammonia, methylamine, ethylamine or a combination thereof.

[0018] In one embodiment of the present invention, the mass ratio of the alkaline gas to the catalyst carrier is 0.008-1.67:1.

[0019] In one embodiment of the present invention, the calcination temperature is 200°C-950°C.

[0020] In one embodiment of the present invention, the sieving mesh size is 10-200 meshes.

[0021] In one embodiment of the present invention, the reduction temperature is 300°C-750°C.

[0022] Another aspect of the present invention provides a device for preparing a carbon nanotube catalyst, the device comprising a spray chamber, a reaction chamber, a calcination section, a screening device, a reduction device and a collecting device, wherein the spray chamber is provided with a catalyst carrier feed port, an active metal salt solution feed device and a stirring device, and the stirring device is located below the catalyst carrier feed port and the active metal salt solution feed device; the reaction chamber is provided with an alkaline gas inlet and a catalyst precursor discharge port, the catalyst precursor discharge port is connected to the calcination section, and the calcination section is connected to the screening device and the reduction device in turn.

[0023] In one embodiment of the present invention, the active metal salt solution feeding device is a spraying device.

[0024] In a preferred embodiment of the present invention, the active metal salt solution feeding device is a multi-nozzle spray device.

[0025] In one embodiment of the present invention, the alkaline gas inlet is located at the bottom of the reaction chamber.

[0026] In one embodiment of the present invention, a gas distributor is provided in the reaction chamber.

[0027] Another aspect of the present invention provides a carbon nanotube catalyst prepared by the method of the present invention.

[0028] Another aspect of the present invention provides a carbon nanotube prepared by using the carbon nanotube catalyst prepared by the method of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The present invention is described below in conjunction with the accompanying drawings.

[0030] In the attached figure:

[0031] Figure 1 is a SEM and EDS scanning image of a carbon nanotube catalyst according to one embodiment of the present invention;

[0032] Figure 2is a SEM image of an array of carbon nanotubes prepared using a carbon nanotube catalyst according to an embodiment of the present invention;

[0033] Figure 3 A device for preparing a carbon nanotube catalyst according to an embodiment of the present invention;

[0034] Figure 4 It is a schematic diagram of a vertical main reactor of a device for preparing a carbon nanotube catalyst according to one embodiment of the present invention;

[0035] Figure 5 It is a schematic diagram of a cyclone-type main reactor of an apparatus for preparing a carbon nanotube catalyst according to one embodiment of the present invention. DETAILED DESCRIPTION

[0036] The method for preparing a carbon nanotube catalyst of the present invention comprises:

[0037] 1) Providing a catalyst carrier and an active metal salt solution;

[0038] 2) infiltrating and mixing the active metal salt solution with the catalyst support;

[0039] 3) introducing alkaline gas into the mixture obtained in step 2) to deposit and age the active metal to prepare a catalyst precursor;

[0040] 4) calcining, screening and reducing the catalyst precursor to prepare a carbon nanotube catalyst.

[0041] The following is a description of the method for preparing the carbon nanotube catalyst:

[0042] In the present invention, the term "carbon nanotube catalyst" refers to a catalyst oxide containing transition metals such as iron, cobalt, and nickel as active metals. The present invention prepares a carbon nanotube catalyst by infiltrating and mixing an active metal salt solution with a catalyst carrier in a spraying or showering manner, then introducing a deposition gas to deposit and age the active metal, and then calcining, screening, and reducing.

[0043] (1) Providing catalyst carrier and active metal salt solution

[0044] In the present invention, the catalyst carrier is a lightweight powder material, a nanomaterial, a porous material, or a lamellar mineral, and may be one of carbon black, graphite, expanded graphite, carbon nanotubes, graphene, vermiculite, alumina, magnesium oxide, gibbsite, hydrotalcite, aluminum hydroxide, calcium hydroxide, mica, and the like, and a combination thereof, preferably vermiculite, gibbsite, and hydrotalcite, and more preferably vermiculite.

[0045] The metal type in the active metal salt solution is a combination of one or more of iron, cobalt, nickel, manganese, vanadium, zinc, copper, molybdenum, magnesium, aluminum, tungsten, calcium, chromium, lanthanum, magnesium, and aluminum, preferably iron, cobalt, nickel, magnesium, and aluminum, and more preferably iron, cobalt, and aluminum; the type of metal salt used is a combination of one or more of nitrate, acetate, sulfate, and chloride, preferably nitrate; the concentration of the active solution is 0.05-10 mol / L, preferably 1-10 mol / L, and more preferably 8-10 mol / L.

[0046] The method for providing the catalyst support and the active metal salt solution of the present invention is not particularly limited and may be any conventional method known in the art.

[0047] In a preferred embodiment of the present invention, the catalyst carrier is vermiculite.

[0048] In a preferred embodiment of the present invention, the active metal salt solution contains iron, cobalt, aluminum and molybdenum.

[0049] (2) mixing the active metal salt solution with the catalyst support

[0050] The active metal salt solution is mixed with the catalyst carrier by spraying or atomizing to achieve infiltration. After the active metal salt solution is mixed with the catalyst carrier by spraying or atomizing, the material is still loose and there is no obvious liquid leaching, so the solid-liquid separation process required after a large amount of solution impregnation can be omitted.

[0051] In the impregnation mixing step, the mixing ratio of the weight of the catalyst support to the weight of the active metal salt solution is 1:0.1-20, preferably 1:0.5-10, more preferably 1:1-5. In this document, unless otherwise specified, the weight of the active metal salt solution refers to the total weight including the solute and the solvent.

[0052] In a preferred embodiment of the present invention, the impregnation mixing is performed under stirring conditions. Preferably, mechanical stirring or gas flow driving is used to achieve sufficient impregnation. The impregnation mixing can also be performed in other forms as long as the active metal salt solution can fully impregnate the catalyst support.

[0053] (3) Passing alkaline gas into the mixture obtained in step 2) to deposit and age the active metal to prepare a catalyst precursor

[0054] An appropriate amount of alkaline gas is introduced into the mixed material fully soaked with the active metal salt solution to deposit and age the active substance. The alkaline gas is introduced so that the alkaline gas and the active metal salt solution loaded on the catalyst carrier can fully, quickly and evenly contact and react, with a short reaction time and excellent effect. The slow release of hydroxide ions in the system is controlled by adjusting the ratio of alkaline gas to active metal salt solution and the gas flow rate, so that the active metal is deposited on the catalyst carrier at an appropriate rate to obtain a catalyst precursor with high uniformity of loading rate and uniform specific surface area. This also avoids the solid-liquid separation operation and the generation of sewage in the process of preparing carbon nanotube catalysts by solution co-precipitation method.

[0055] On the other hand, when the alkaline gas is introduced for precipitation, a large amount of heat is released due to the alkaline gas dissolving in water and the acid-base neutralization effect. Under the stirring action, this heat quickly evaporates the previous infiltration solution to achieve a drying effect. At the same time, the thermal effect also accelerates the aging of the precipitate.

[0056] In a preferred embodiment of the present invention, the alkaline gas is selected from ammonia, methylamine, ethylamine or a combination thereof; preferably ammonia.

[0057] In a preferred embodiment of the present invention, the weight ratio of the alkaline gas to the catalyst carrier is 0.008-1.67:1.

[0058] In a preferred embodiment of the present invention, the weight ratio of the alkaline gas to the active metal salt solution is 0.8:1, preferably 0.8-1.2:1.

[0059] 4) calcining, screening and reducing the catalyst precursor to prepare a carbon nanotube catalyst

[0060] The calcination, screening and reduction of the catalyst precursor may be carried out in any appropriate manner known in the art.

[0061] In one embodiment of the present invention, the calcination temperature is 200°C-950°C, preferably 450°C-650°C, most preferably 450°C; the sieving mesh is 10-200 mesh, preferably 20-40 mesh; the reduction temperature is 300°C-750°C, preferably 550-650°C.

[0062] The device for preparing a carbon nanotube catalyst of the present invention comprises a spray chamber, a reaction chamber, a calcination section, a screening device and a reduction device, wherein the spray chamber is provided with a catalyst carrier feed port, an active metal salt solution feed device and a stirring device, the stirring device is located below the catalyst carrier feed port and the active metal salt solution feed device, the spray chamber is connected with the reaction chamber; the reaction chamber is provided with an alkaline gas inlet and a catalyst precursor discharge port, the catalyst precursor discharge port is connected with the calcination section, and the calcination section is connected with the screening device and the reduction device in sequence.

[0063] The specific components of the device for preparing carbon nanotube catalyst are described below:

[0064] The preparation of carbon nanotube catalyst precursor is carried out in a reactor including a spray chamber and a reaction chamber. The reactor is provided with a catalyst carrier feed port, an active metal salt solution feed device, a stirring device, an alkaline gas inlet and a catalyst precursor discharge port.

[0065] The catalyst carrier feed port is located at the upper part of the reactor and is connected to the spray chamber. The catalyst carrier can be stored in a carrier storage tank and enter the spray chamber through the catalyst carrier feed port. The active metal salt solution can be stored in an active metal salt solution storage tank and enter the spray chamber through an active metal salt solution feeding device. The catalyst carrier can adsorb the solution by adjusting and controlling the liquid spraying amount of the feeding device. The stirring device is located below the catalyst carrier feed port and the active metal salt solution feeding device, and the catalyst carrier is stirred by mechanical stirring or gas flow to promote sufficient infiltration. After the active metal salt solution and the catalyst carrier are mixed in the form of spraying or atomizing, the material is still loose, and there is no obvious liquid leaching. When there is no liquid on the surface of the material by visual observation, the material enters the reaction chamber to react with the alkaline gas.

[0066] In a preferred embodiment, the active metal salt solution feeding device is a spray device, and the spray device is preferably a multi-nozzle spray device. In a preferred embodiment, the stirring device is a mechanical stirring form.

[0067] The reaction chamber is provided with an alkaline gas inlet and a catalyst precursor outlet, and the alkaline gas inlet can be selectively arranged at one or more locations of the bottom, middle, top, one side or any position of the reaction chamber.

[0068] In a preferred embodiment, the alkaline gas is selected from ammonia, methylamine, ethylamine or a combination thereof; preferably ammonia. In a preferred embodiment, the alkaline gas inlet is located at the bottom of the reaction chamber. In a preferred embodiment, the reaction chamber is also provided with a gas distributor to facilitate the full progress of the reaction. The weight ratio of the introduction ratio of the alkaline gas to the catalyst carrier is 0.008-1.67:1, preferably 0.8-1.2:1. The weight ratio of the alkaline gas to the active metal salt solution is 0.0064-1.944:1, preferably 0.8-6:1.

[0069] The spray chamber and the reaction chamber can be arranged separately or integrated together. The reaction chamber can be of horizontal, vertical or cyclone structure.

[0070] In the present invention, there is no particular restriction on the type of the catalyst carrier feed port and the active metal salt solution feed device, as long as it is a feed device suitable for feeding the catalyst carrier and the active metal salt solution. The feed device can be arranged horizontally or vertically. There is no particular restriction on the type of the stirring device, as long as it can achieve the purpose of sufficient stirring and mixing.

[0071] The catalyst precursor discharge port is connected to the calcination section, and the catalyst precursor formed by the reaction enters the calcination section through the catalyst precursor discharge port. The calcination section is sequentially arranged in series with the screening device and the reduction device. The catalyst precursor enters the calcination device from the discharge port of the reaction chamber, enters the screening device for screening with a specific mesh after high-temperature calcination, and then enters the reduction device for reduction activation, thereby preparing a carbon nanotube catalyst.

[0072] The present invention has no particular restrictions on the calcination device, screening device and reduction device, as long as the conditions required for calcination, screening and reduction can be provided. The screening, reduction and activation of the catalyst precursor can be set independently or integrated together.

[0073] In a preferred embodiment of the present invention, the calcining section is a roller furnace; the screening device is a vibrating screen; and the reduction device is a reduction kettle.

[0074] In one embodiment of the present invention, the calcination temperature of the calcination stage is 200°C-950°C, preferably 450°C; the screening mesh of the screening device is 10-200 mesh, preferably 20-40 mesh; the reduction temperature of the reduction device is 300°C-750°C, preferably 550-650°C.

[0075] The carbon nanotube catalyst prepared by the method of the present invention has high uniformity in loading rate, stable data such as specific surface area, and improved real catalytic activity multiple. The process of the present invention is simple, the conditions are easy to control, the product stability is good, the production efficiency is significantly improved, and continuous batch production can be realized.

[0076] The carbon nanotube catalyst prepared by the method of the present invention can be used to prepare carbon nanotubes through a chemical vapor deposition method. The prepared carbon nanotubes have a thin diameter and a narrow distribution, good electrical conductivity and a large specific surface area.

[0077] The specific implementation of the present invention is described in detail below with reference to the accompanying drawings:

[0078] Figure 3 It is a schematic diagram of a horizontal device for preparing a carbon nanotube catalyst in a preferred embodiment of the present invention.

[0079] Figure 3 The device for preparing carbon nanotube catalyst shown in the figure comprises a catalyst carrier feed port 1, a carrier storage tank 2, an active metal salt solution feed device 3, an active metal salt solution storage tank 4, a stirring device 5, a spray chamber 6, a reaction chamber 7, an alkaline gas inlet 8, an alkaline gas storage tank 9, a gas distributor 10, a catalyst precursor discharge port 11, a tail gas absorption device 12, a calcination section 13, a screening device 14, a reduction device 15 and a discharge port 16. The catalyst carrier feed port 1 and the active metal salt solution feed device 3 are arranged at the upper part of the spray chamber 6, above the stirring device 5, the alkaline gas inlet 8 is arranged at the bottom of the reaction chamber 7, a gas distributor 10 is arranged in the reaction chamber, the catalyst precursor discharge port 11 is connected to the calcination section 13, and the calcination section 13 is sequentially connected to the separation device 14, the reduction device 15 and the discharge port 16.

[0080] use Figure 3 In the reaction device shown, the catalyst carrier from the carrier storage tank 2 is quantitatively loaded into the spray chamber 6 from the catalyst carrier feed port 1, the active metal salt solution from the active metal salt solution storage tank 4 enters the spray chamber 6 through the active metal salt solution feed device 3, the catalyst carrier is fully infiltrated and mixed with the active metal salt solution under the action of the stirring device 5, and then enters the reaction chamber 7, the alkaline gas from the alkaline gas storage tank 9 enters the reaction chamber 7 through the alkaline gas inlet 8 through the gas distributor 10, and reacts with the catalyst carrier fully infiltrated with the active metal salt solution in the reaction chamber 7. The catalyst precursor obtained by the reaction enters the calcination section 13 through the catalyst precursor discharge port 11, and the tail gas is removed by the tail gas absorption device 12. After calcination, the catalyst precursor enters the screening device 14 for screening of a specific mesh number, and then enters the reduction device 15 for reduction activation to prepare a carbon nanotube catalyst, which is discharged through the discharge port 16.

[0081] Figure 4 It is a partial schematic diagram of a vertical reaction device for preparing carbon nanotube catalysts in a preferred embodiment of the present invention.

[0082] Figure 4The spray chamber and reaction chamber for preparing carbon nanotube catalysts are integrated in a vertical reaction device. The vertical reaction device includes a catalyst carrier feed port 1, an exhaust port 2, an active metal salt solution feed device 3, an alkaline gas inlet 4, a stirring device 5, and a catalyst precursor discharge port 6. The catalyst carrier feed port 1 and the active metal salt solution feed device 3 are arranged at the upper part of the reaction device, above the stirring device 5, the alkaline gas inlet 4 is arranged at the upper part, middle part and bottom part of the reactor, and the catalyst precursor discharge port 6 is connected to the calcination section ( Figure 4 Not shown) connected.

[0083] use Figure 4 In the reaction device shown, the catalyst carrier is quantitatively loaded into the reaction device from the catalyst carrier feed port 1, the active metal salt solution enters the reaction device through the active metal salt solution feed device 3, the catalyst carrier is fully infiltrated and mixed with the active metal salt solution under the action of the stirring device 5, the alkaline gas enters the reaction device from the alkaline gas inlet 4, and reacts with the catalyst carrier fully infiltrated with the active metal salt solution under the action of the stirring device 5. The alkaline gas inlet 4 is respectively arranged at the top, middle and bottom of the reactor to facilitate uniform distribution of the intake air. The catalyst precursor obtained by the reaction enters the calcination section through the catalyst precursor discharge port 6, and the tail gas is discharged through the tail gas exhaust port 2. The subsequent calcination section, screening device and reduction device are Figure 3 The same is not repeated here.

[0084] Figure 5 It is a partial schematic diagram of a cyclone reaction device for preparing carbon nanotube catalysts in a preferred embodiment of the present invention.

[0085] Figure 5 The spray chamber and reaction chamber for preparing carbon nanotube catalysts are integrated in a cyclone reaction device. The cyclone reaction device includes a catalyst carrier and alkaline gas inlet 1, an exhaust gas outlet 2, an active metal salt solution feed device 3, a mixing area 4, and a catalyst precursor outlet 5, wherein the catalyst carrier feed port and the alkaline gas inlet are set to the same inlet, the active metal salt solution feed device 3 is set at the upper part of the reaction device, located above the mixing area 4, and the catalyst precursor outlet 5 is connected to the calcination section ( Figure 4 Not shown) connected.

[0086] use Figure 5In the reaction device shown in the figure, the catalyst carrier is quantitatively loaded into the reaction device from the inlet 1, the active metal salt solution enters the reaction device through the active metal salt solution feeding device 3, the catalyst carrier is fully infiltrated and mixed with the active metal salt solution in the mixing area 4, and the alkaline gas also enters the reaction device from the inlet 1, and reacts with the catalyst carrier fully infiltrated with the active metal salt solution in the mixing area 4. The catalyst precursor obtained by the reaction enters the calcination section through the catalyst precursor discharge port 5, and the tail gas is discharged through the tail gas exhaust port 2. The subsequent calcination section, screening device and reduction device are Figure 3 The same is not repeated here.

[0087] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. For the experimental methods in the following examples where specific conditions are not specified, conventional conditions are usually used, or the conditions recommended by the manufacturer. Ratios and percentages are based on molar amounts unless otherwise specified.

[0088] Raw material source and preparation:

[0089] (1) Catalyst carrier:

[0090] 20-40 mesh vermiculite, a product of Lingshou County Dongbai Mineral Products Vermiculite Processing Plant Co., Ltd., No.: 06;

[0091] 80-100 mesh vermiculite, a product of Lingshou County Dongbai Mineral Products Vermiculite Processing Plant Co., Ltd., No.: 10;

[0092] 80-100 mesh expanded graphite, a product of Qingdao Coastal Carbon Materials Co., Ltd., No.: YH-100;

[0093] 120-200 mesh diaspore, product of China Aluminum Shandong Co., Ltd., No.: H-BD-9995-1.

[0094] (2) Active metal salt solution:

[0095] The preparation method of the iron, cobalt and aluminum active metal salt solution is as follows: 20g of ferric nitrate nonahydrate, 3g of cobalt nitrate hexahydrate and 45g of aluminum nitrate nonahydrate are added to 40g of deionized water in sequence and stirred until completely dissolved;

[0096] The preparation method of the iron, nickel and magnesium active metal salt solution is as follows: 20g of ferric nitrate nonahydrate, 15g of nickel nitrate hexahydrate and 32g of magnesium nitrate hexahydrate are sequentially added into 40g of deionized water and stirred until completely dissolved;

[0097] The cobalt, manganese, magnesium and aluminum active metal salt solution is prepared by sequentially adding 14 g of cobalt nitrate hexahydrate, 20 g of manganese nitrate aqueous solution (50% by mass), 18 g of magnesium nitrate hexahydrate and 18 g of aluminum nitrate nonahydrate into 100 g of deionized water and stirring until they are completely dissolved;

[0098] The cobalt-vanadium active metal salt solution is prepared by sequentially adding 25 g of cobalt nitrate hexahydrate and 13 g of ammonium metavanadate into 100 g of deionized water and stirring until the solution is completely dissolved.

[0099] (3) Alkaline gas:

[0100] Ammonia was purchased from Zouping Jinhe Chemical Co., Ltd.

[0101] Methylamine was purchased from Nantong Jiuwu Chemical Co., Ltd.;

[0102] The preparation method of 8% ammonia solution is as follows: dilute 100g of 17% ammonia solution with 112.5g of deionized water and stir evenly.

[0103] Preparation Example 1:

[0104] (1) Add 20-40 mesh vermiculite into the carrier storage tank and continuously add it into the spray chamber at 50 kg / h through a quantitative filling device;

[0105] (2) preparing an active metal salt solution of iron, cobalt and aluminum with a concentration of 1.7 mol / L and a molar ratio of 4:1:6, and continuously mixing it with vermiculite in the form of spray from a solution storage tank at a rate of 80 kg / h, and achieving uniform infiltration through stirring;

[0106] (3) After the material fully soaked with the active metal salt solution enters the reaction chamber, ammonia gas is introduced through the gas distributor at a rate of 6.25 kg / h from the bottom vent, and the ammonia gas reacts with the soaked material by stirring, depositing and aging the active material to form a catalyst precursor;

[0107] (4) The calcination section is pre-heated to 640°C to calcine the catalyst precursor at high temperature, and the frequency conversion is set so that the calcination time is 180 min;

[0108] (5) After the calcined material is cooled, it is continuously screened on a vibrating screen, and the screen size is set to 20 meshes;

[0109] (6) The temperature of the reduction kettle was preheated to 500° C., and hydrogen was intermittently passed through the reduction kettle at a rate of 60 kg / h to activate the catalyst precursor, thereby continuously preparing the catalyst.

[0110] Preparation Example 2:

[0111] (1) Add 80-100 mesh vermiculite into the carrier storage tank and continuously add it into the spray chamber at 60 kg / h through a quantitative filling device;

[0112] (2) preparing an active metal salt solution of iron, nickel and magnesium with a concentration of 3.2 mol / L and a molar ratio of 3:1:6, and continuously mixing it with vermiculite in the form of spray from a solution storage tank at a speed of 120 kg / h, and achieving uniform infiltration through stirring;

[0113] (3) After the material fully soaked with the active metal salt solution enters the reaction chamber, ammonia gas is introduced through the gas distributor at a rate of 8.53 kg / h from the bottom vent, and the ammonia gas reacts with the soaked material by stirring, depositing and aging the active material to form a catalyst precursor;

[0114] (4) The calcination section is pre-heated to 550° C. to calcine the catalyst precursor at high temperature, and the frequency conversion is set so that the calcination time is 150 min;

[0115] (5) After the calcined material is cooled, it is continuously screened on a vibrating screen, and the screen size is set to 80 meshes;

[0116] (6) The temperature of the reduction kettle was preheated to 620° C., and hydrogen was intermittently passed into the reduction kettle at a rate of 75 kg / h to activate the catalyst precursor, thereby continuously preparing the catalyst.

[0117] Preparation Example 3:

[0118] (1) Add 80-100 mesh expanded graphite into the carrier storage tank, and continuously add it into the spray chamber at 20 kg / h through a quantitative filling device;

[0119] (2) preparing a cobalt, manganese, magnesium, and aluminum active metal salt solution with a concentration of 0.85 mol / L and a molar ratio of 1:1:2:2, and continuously mixing it with vermiculite in the form of spray from a solution storage tank at a speed of 75 kg / h, and achieving uniform infiltration through stirring;

[0120] (3) After the material fully soaked with the active metal salt solution enters the reaction chamber, ammonia gas is introduced through the gas distributor at a rate of 3.27 kg / h from the bottom vent, and the ammonia gas reacts with the soaked material by stirring, depositing and aging the active material to form a catalyst precursor;

[0121] (4) The calcination section is pre-heated to 530° C. to calcine the catalyst precursor at high temperature, and the frequency conversion is set so that the calcination time is 120 min;

[0122] (5) After the calcined material is cooled, it is continuously screened on a vibrating screen with a screen size of 100 meshes;

[0123] (6) The temperature of the reduction kettle was preheated to 470° C., and hydrogen was intermittently passed into the reduction kettle at a rate of 32 kg / h to activate the catalyst precursor, thereby continuously preparing the catalyst.

[0124] Preparation Example 4:

[0125] (1) Add 120-200 mesh diaspore to the carrier storage tank and continuously add it into the spray chamber at 15 kg / h through a quantitative filling device;

[0126] (2) preparing a cobalt-vanadium active metal salt solution with a concentration of 0.36 mol / L and a molar ratio of 7:1, and continuously mixing it with vermiculite in the form of spray from a solution storage tank at a speed of 24 kg / h, and achieving uniform infiltration through stirring;

[0127] (3) After the material fully soaked with the active metal salt solution enters the reaction chamber, methylamine is introduced through the bottom vent at a rate of 2.4 kg / h through the gas distributor, and the methylamine reacts with the soaked material by stirring, depositing and aging the active material to form a catalyst precursor;

[0128] (4) The calcination section is pre-heated to 350° C. to calcine the catalyst precursor at high temperature, and the frequency conversion is set so that the calcination time is 200 min;

[0129] (5) After the calcined material is cooled, it is continuously screened on a vibrating screen with a screen size of 200 meshes;

[0130] (6) The temperature of the reduction kettle was preheated to 500° C., and hydrogen was intermittently passed into the reduction kettle at a rate of 18.5 kg / h to activate the catalyst precursor, thereby continuously preparing the catalyst.

[0131] Comparative Example 1:

[0132] Prepare 30 kg of active metal salt solution of iron, cobalt and aluminum with a concentration of 1.7 mol / L and a molar ratio of 4:1:6;

[0133] (2) Add 5 kg of 20-40 mesh vermiculite to the active solution, stir evenly and let stand for 12 hours;

[0134] (3) The material is filtered and the filter cake is dried in an oven at 120°C;

[0135] (4) roasting the dried material in a roller furnace, setting the roasting temperature to 640°C and the roasting time to 180 min;

[0136] (5) After the calcined material is cooled, it is sieved through a 20-mesh sieve;

[0137] (6) The catalyst precursor was reduced in a reduction reactor at 500° C. to prepare comparative catalyst 1.

[0138] Comparative Example 2:

[0139] (1) preparing 30 kg of an active metal salt solution of iron, cobalt and aluminum having a concentration of 1.7 mol / L and a molar ratio of 4:1:6;

[0140] (2) Add 5 kg of 20-40 mesh vermiculite to the active solution, stir evenly and let stand for 12 hours;

[0141] (3) Prepare 18.75 kg of 8% ammonia solution and slowly add it dropwise to the above-mentioned impregnated material while stirring;

[0142] (4) The material is filtered and the filter cake is dried in an oven at 120°C;

[0143] (5) roasting the dried material in a roller furnace, setting the roasting temperature to 640°C and the roasting time to 180 min;

[0144] (6) After the calcined material is cooled, it is sieved through a 20-mesh sieve;

[0145] (7) The catalyst precursor was reduced in a reduction reactor at 500°C to prepare comparative catalyst 2.

[0146] Product performance test:

[0147] (1) Microscopic morphology test:

[0148] The carbon nanotube catalyst prepared in Example 3 of the present invention was observed by scanning electron microscopy (SEM). The SEM photo results are shown in Figure 1 (left); elemental analysis was performed by EDS scanning electron microscopy, and the results are shown in Figure 1 (Right) The active metal elements in the prepared catalyst are magnesium, aluminum, manganese and cobalt. The specific surface area of ​​the catalyst is measured using a specific surface area tester.

[0149] (2) Catalytic effect:

[0150] Carbon nanotubes are prepared using the carbon nanotube catalyst prepared in Example 1 of the present invention:

[0151] 2 g of the catalyst prepared in Example 1 was added to a quartz fluidized bed reactor with a diameter of 50 mm. The reactor was heated to 690° C. under a nitrogen atmosphere. The nitrogen flow rate was adjusted to 150 L / h, the hydrogen flow rate was 50 L / h, and the propylene flow rate was 50 L / h. The reaction lasted for 60 min. After the reaction was completed, the heating was stopped, the hydrogen and propylene were turned off, and the nitrogen atmosphere was maintained. After the temperature was naturally cooled to room temperature, the material was unloaded to obtain 44 g of array carbon nanotube products with a growth rate of 22 times. Its SEM photo is shown in Figure 2 .from Figure 2 It can be seen that the array carbon nanotubes prepared by the method of the present invention have the characteristics of high array ratio, less tortuosity in carbon tube growth and good oriented morphology.

[0152] The same process was followed to prepare carbon nanotubes using the comparative catalysts 1 and 2 obtained in comparative examples 1 and 2. The obtained carbon nanotube products were tested for specific surface area, carbon tube growth rate, and carbon tube resistivity using a specific surface area tester and a four-probe resistivity tester. The data results are summarized in the following table:

[0153]

[0154] It can be seen from the above data results that the carbon nanotube catalyst prepared by the method of the present invention has the advantages of high uniformity of loading rate, large specific surface area, and high real catalytic activity multiple; the carbon nanotube catalyst prepared by the present invention has a fine diameter and a narrow distribution of carbon nanotubes prepared by CVD, good conductivity, large specific surface area, and excellent performance, which can meet the needs of commercial applications and is suitable for industrial large-scale production.

[0155] The process method for preparing carbon nanotube catalysts of the present invention, the amount of raw materials used and the process parameters are not limited to the above-mentioned embodiments. After reading the above teachings of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A method for preparing a carbon nanotube catalyst, the method comprising: 1) providing a catalyst carrier and an active metal salt solution, wherein the carrier is vermiculite; 2) infiltration and mixing the active metal salt solution with the catalyst support, wherein the infiltration and mixing is carried out in the form of spraying or atomizing; 3) introducing alkaline gas into the mixture obtained in step 2) to deposit and age the active metal to prepare a catalyst precursor, wherein the weight ratio of the alkaline gas to the active metal salt solution is 0.8-1.2:1; 4) calcining, screening and reducing the catalyst precursor to prepare a carbon nanotube catalyst.

2. The method according to claim 1, wherein in the infiltration and mixing step, the mixing mass ratio of the catalyst support to the active metal salt solution is 1:0.1-20.

3. The method of claim 1, wherein the active metal salt solution comprises one or more metals selected from iron, cobalt, nickel, manganese, vanadium, zinc, copper, molybdenum, magnesium, aluminum, tungsten, calcium, chromium, and lanthanum; and / or the metal salt is a combination of one or more of nitrate, acetate, sulfate, and chloride; and / or The concentration of the active metal salt solution is 0.05-10 mol / L.

4. The method of claim 1, wherein the alkaline gas is selected from ammonia, methylamine, ethylamine or a combination thereof; and / or The mass ratio of the alkaline gas to the catalyst carrier is 0.008-1.67:

1.

5. The method according to claim 1, wherein the calcination temperature is 200°C-950°C; the sieving mesh is 10-200 mesh; and the reduction temperature is 300°C-750°C.

6. A device for the method of preparing a carbon nanotube catalyst as described in claim 1, the device comprising a spray chamber, a reaction chamber, a calcination section, a screening device, a reduction device and a collecting device, wherein the spray chamber is provided with a catalyst carrier feed port, an active metal salt solution feed device, and a stirring device, and the stirring device is located below the catalyst carrier feed port and the active metal salt solution feed device; the reaction chamber is provided with an alkaline gas inlet and a catalyst precursor outlet, the catalyst precursor outlet is connected to the calcination section, and the calcination section is connected to the screening device and the reduction device in turn, and the alkaline gas inlet is located at the bottom of the reaction chamber.

7. The device as claimed in claim 6, wherein the active metal salt solution feeding device is a spraying device.

8. The device as claimed in claim 7, wherein the spray device is a multi-nozzle spray device.

9. The device as claimed in claim 6, wherein a gas distributor is provided in the reaction chamber.

10. A carbon nanotube catalyst prepared according to the method of claim 1.

11. A carbon nanotube prepared by using the carbon nanotube catalyst prepared by the method according to claim 1.