A method for improving photoresist bleaching during wafer development
By using HMDS adhesive film to protect the photoresist strip during the photoresist development process, the problems of photoresist bleeding and tilting caused by centrifugal force during spin drying are solved, the aspect ratio of the photoresist strip is improved, and the stability of the photoresist morphology and the quality of subsequent processes are ensured.
Patent Information
- Application Number
- CN202111368347.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-18
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2041-11-18
Smart Images

Figure CN116136651B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of power semiconductor device fabrication technology, and specifically relates to a method for improving photoresist bleaching during wafer development. Background Technology
[0002] A wafer refers to a silicon wafer or other semiconductor material wafer used in the fabrication of semiconductor integrated circuits. It is called a wafer because of its circular shape. Various circuit element structures can be fabricated on silicon wafers to create IC products with specific electrical functions.
[0003] For positive photoresist, the development process involves dissolving and removing the photoresist in the exposed areas after wafer coating and exposure, forming a mask pattern on the photoresist film. This is an essential step in photolithographic pattern transfer and has a crucial impact on the formation of high-quality patterns. The developer is a chemical solvent that dissolves the soluble areas of the photoresist caused by exposure. The most common and widely used is tetramethylammonium hydroxide (TMAH). However, with increasingly stringent requirements for linewidth and uniformity in photolithography, the photolithography field is attempting to modify existing TMAH developers.
[0004] The aspect ratio of a photoresist pattern refers to the ratio between the height of the photoresist strip in the vertical direction and its width in the horizontal direction (e.g., ...). Figure 1 (As shown). For photoresist of the same thickness, a larger lateral width results in a larger contact area with the wafer surface, meaning better adhesion. In practice, to etch finer lines on the wafer, the photoresist strip often needs to be very thin. Considering the etching ratio between the wafer and the photoresist, there is a critical thickness for the photoresist mask layer; it cannot be lower than this thickness, meaning the aspect ratio of the photoresist strip needs to be very large.
[0005] Currently, the development methods vary depending on the equipment. Most production lines have phased out the manual immersion and vibration development method, adopting a process of immersion followed by rotation and spin-drying, and then rinsing with deionized water. However, this method also has certain drawbacks. For photoresist strips with a large aspect ratio, high-speed rotation can cause the strip to fly away due to excessive centrifugal force, or the photoresist morphology to tilt in the direction of centrifugal force (e.g., Figure 2-4 As shown in the diagram, the photoresist surface also absorbs the developer and deionized water, further increasing the centrifugal force at the top of the photoresist strip. Therefore, the aspect ratio has a significant impact on most current development processes, which in turn affects the morphology of the photoresist and determines the quality of subsequent wafer etching or ion implantation processes. Summary of the Invention
[0006] To overcome the shortcomings of existing technologies, this invention provides a method for improving photoresist bleaching during wafer development, comprising the following steps:
[0007] (1) Place the wafer in an oven with an HMDS atmosphere to form an HMDS film with a thickness of 5 to 30 nanometers on the wafer surface as a photoresist adhesive.
[0008] (2) A photoresist film is spin-coated onto the HMDS film already formed on the wafer surface, and then dried and cured;
[0009] (3) Expose the photoresist film using a step-scan I-line lithography machine;
[0010] (4) Rotate and wash the wafer surface, rotate and spread the developer solution to all areas of the photoresist film surface and immerse it, rotate and shake off the developer solution, and rotate and wash again.
[0011] Repeat steps (1) and (4).
[0012] In steps (3) and (4), after exposure, the molecular structure and van der Waals forces of the photoresist are damaged, and micro-gaps are formed in the photoresist, making it susceptible to etching or dissolution by the developer. Step (1) is executed again, but a continuous HMDS film cannot form in the exposed area, while a continuous HMDS film forms on the upper surface and sidewalls of the unexposed area (i.e., the photoresist strip). Then, step (4) is executed. On the one hand, because the HMDS film in the exposed area is discontinuous, the developer dissolves the remaining photoresist in the exposed area more quickly. Conversely, due to the protection of the continuous HMDS film, the developer dissolves the upper surface and sidewalls of the photoresist strip much more slowly. On the other hand, the continuous HMDS film on the upper surface and sidewalls of the photoresist strip helps it resist washing and immersion in water, while also providing mechanical reinforcement to prevent centrifugal force from causing photoresist bleed-off. Therefore, the aspect ratio of the photoresist strip is improved.
[0013] Preferably, the temperature in the oven in step (1) is 110-130°C and the baking time is 110-130 seconds.
[0014] Preferably, the temperature in the oven in step (1) is 120±1℃ and the baking time is 120 seconds.
[0015] Preferably, AZ MIR-703 photoresist is used in step (2), and the thickness of the photoresist film ranges from 1.8 to 2.1 micrometers.
[0016] Preferably, AZ MIR-6130 photoresist is used in step (2), and the photoresist film thickness ranges from 2.8 to 6 micrometers.
[0017] Preferably, in step (3): the exposure time is 345±15 milliseconds, the focal length range is -0.2 to 0.2, the light intensity is 650 to 750 mW / cm², the light intensity non-uniformity of the exposure area is less than 2%, and the narrowest line width of the photomask is 0.35±0.05 micrometers.
[0018] More preferably, the exposure time is 345 milliseconds.
[0019] Preferably, in step (4): the exposed wafer surface is rotated and rinsed with water for 20±2 seconds, the developer is rotated and spread to all areas of the photoresist film surface, soaked for 15 to 20 seconds, the developer is shaken off by rotating at 300±50 rpm for 5±1 seconds, and then the wafer surface is rotated and rinsed with water for 20±2 seconds by rotating at 300±50 rpm.
[0020] More preferably, in step (4): the exposed wafer surface is rotated and rinsed with water for 20 seconds, the developer is rotated and spread to all areas of the photoresist film surface, soaked for 15 seconds, the developer is shaken off by rotating at 300 rpm for 5 seconds, and then the wafer surface is rotated and rinsed with water for 20 seconds by rotating at 300 rpm.
[0021] Preferably, the thickness of the HMDS mucosa formed in step (1) is 10 to 20 nanometers.
[0022] Preferably, step (1) or its preferred embodiment and step (4) or its preferred embodiment are repeated 2-4 times.
[0023] Preferably, step (1) or its preferred embodiment and step (4) or its preferred embodiment are repeated three times.
[0024] The technical solution of the present invention improves or avoids the photoresist bleed caused by centrifugal force by repeating steps (1) and (4) for multiple developments, thereby increasing the aspect ratio of the photoresist strip. Attached Figure Description
[0025] Figure 1 A schematic diagram of the aspect ratio of photoresist strips;
[0026] Figure 2 It is a scanning electron microscope image of the photoresist bleaching surface;
[0027] Figure 3 It is a scanning electron microscope image of the tilted surface of the adhesive strip;
[0028] Figure 4 It is a scanning electron microscope image (aspect ratio 3.2) of the oblique cross-section of the adhesive strip morphology;
[0029] Figure 5 These are scanning electron microscope images of the surface of the photoresist lines using a preferred embodiment of the present invention;
[0030] Figure 6 These are scanning electron microscope images of the cross-sectional morphology of the adhesive strip according to a preferred embodiment of the present invention;
[0031] Figure 7 This is a scanning electron microscope image of the morphology of the adhesive strip with an aspect ratio of 5.3 according to a more preferred embodiment of the present invention (height H: width L = 1.75 μm: 0.33 μm = 5.3). Detailed Implementation
[0032] To better understand this invention, the following will be discussed in conjunction with the accompanying drawings. Figure 5-7 The following experimental results further illustrate the content of this invention. Among them, Figure 6 From Figure 5 The enlarged cross-sectional morphology of the adhesive strip in the middle section; especially Figure 7 The aspect ratio of the adhesive strip is 5.3, that is, (height H: width L) = (1.75 micrometers: 0.33 micrometers) = 5.3.
[0033] This invention relates to a method for improving photoresist bleaching during wafer development, comprising the following steps:
[0034] (1) The wafer is placed in an oven with an HMDS (hexamethyldisilazane) atmosphere to form an HMDS film with a thickness of 5 to 30 nanometers (preferably 10 to 20 nanometers) on the wafer surface as a photoresist adhesive; that is, the HMDS film is deposited on the wafer surface by diffusion and transition in the HMDS atmosphere and accumulates to form an HMDS film. The HMDS film is the photoresist adhesive of the present invention, that is, a photoresist adhesive made of HMDS, and its purpose is to adhere the photoresist more firmly (as described in step (2) below).
[0035] (2) A photoresist film is spin-coated onto the HMDS film already formed on the wafer surface, and then dried and cured. In this specific embodiment, the photoresist used is AZ MIR-703 or AZ MIR-6130, but these are only two specific embodiments of the photoresist and do not limit the scope of the present invention. The drying temperature can be 110-130°C, and the drying time can be 110-130 seconds.
[0036] (3) Expose the photoresist film using a step-scan I-line lithography machine; the purpose of using a step-scan I-line lithography machine is to increase the aspect ratio of the photoresist strip, that is, to reduce the width of the photoresist strip.
[0037] (4) The wafer surface is rotated and rinsed with water to remove the surface tension of the photoresist film (also known as the photoresist film or photoresist film), so that the developer can cover all areas of the photoresist film surface; the developer is rotated and applied to all areas of the photoresist film surface and then immersed to dissolve the exposed pattern or part of the photoresist film; the developer is then rotated and shaken off, and the remaining developer is rinsed with water again. In this specific embodiment, FHD-5 developer is used, but this is only one specific embodiment of the developer and does not limit the scope of the invention; the water used for rinsing is usually deionized water.
[0038] Repeat steps (1) and (4). That is, after completing step (4), perform step (1) again, placing the wafer in an oven with an HMDS (hexamethyldisilazane) atmosphere to form an HMDS film with a thickness of 5-30 nanometers (preferably 10-20 nanometers) on the wafer surface. At this time, an HMDS film is formed on the photoresist strip and the exposure area. In steps (3) and (4), after the photoresist is exposed, the molecular structure and van der Waals forces are damaged, and micro-gaps are formed in the photoresist, making it easy to be etched or dissolved by the developer. When step (1) is performed again, a continuous HMDS film cannot be formed in the exposure area, but a continuous HMDS film is formed on the upper surface and sidewalls of the unexposed area (i.e., the photoresist strip). Then, step (4) is performed: the wafer surface is rotated and rinsed with water; the developer is rotated to cover all areas of the photoresist film surface and immersed in it; the developer is rotated and spun off; and then rotated and rinsed again. Because the HMDS film in the exposure area is discontinuous, the developer dissolves the photoresist still present in the exposure area more quickly. Conversely, due to the protection of the continuous HMDS film, the developer dissolves the upper surface and sidewalls of the photoresist strip much more slowly. On the other hand, the continuous HMDS film on the upper surface and sidewalls of the photoresist strip helps the photoresist strip resist water washing and immersion, and also provides mechanical reinforcement to prevent the photoresist from floating due to centrifugal force. Therefore, the aspect ratio of the photoresist strip is improved.
[0039] In an optional embodiment, the temperature in the oven in step (1) is 110-130°C and the baking time is 110-130 seconds.
[0040] In a preferred embodiment, the temperature in the oven in step (1) is 120±1℃ and the baking time is 120 seconds.
[0041] In an optional embodiment, AZ MIR-703 photoresist is used in step (2), and the photoresist film thickness ranges from 1.8 to 2.1 micrometers.
[0042] In an optional embodiment, AZ MIR-6130 photoresist is used in step (2), and the photoresist film thickness ranges from 2.8 to 6 micrometers.
[0043] In an optional embodiment, the exposure time in step (3) is 345±15 milliseconds, the focal length range is -0.2 to 0.2, the light intensity is 650 to 750 mW / cm², the light intensity non-uniformity of the exposure area is less than 2%, and the narrowest line width of the photomask is 0.35±0.05 micrometers.
[0044] In a preferred embodiment, the exposure time is 345 milliseconds.
[0045] In one optional embodiment, the exposed wafer surface is rotated and rinsed with water for 20±2 seconds, the developer is rotated to cover all areas of the photoresist film surface, and after soaking for 15 to 20 seconds, the developer is removed by rotating at 300±50 rpm for 5±1 seconds, and then the wafer surface is rotated and rinsed with water at 300±50 rpm for 20±2 seconds.
[0046] In one optional embodiment, the exposed wafer surface is rotated and rinsed with water for 20 seconds, the developer is rotated to cover all areas of the photoresist film surface, soaked for 15 seconds, the developer is shaken off by rotating at 300 rpm for 5 seconds, and then the wafer surface is rotated and rinsed with water for 20 seconds by rotating at 300 rpm.
[0047] In an optional embodiment, steps (1) and (4) are repeated 2-4 times.
[0048] In a preferred embodiment, steps (1) and (4) are repeated three times.
[0049] Preferred embodiment 1
[0050] A method for improving photoresist bleaching during wafer development includes the following steps:
[0051] (1) Place the silicon carbide wafer in an HMDS atmosphere oven at 110°C for 110 seconds to form an HMDS film with a thickness of 5-10 nanometers on the wafer surface as a photoresist adhesive; the purpose is to obtain a larger aspect ratio of the photoresist strips, which is actually to make grooves between narrower and deeper photoresist strips.
[0052] (2) Spin-coat an AZ MIR-6130 photoresist film onto the HMDS film already formed on the wafer surface, and then dry and cure it; cure in an oven at 120°C for 120 seconds.
[0053] (3) The photoresist film is exposed using a step-scan I-line lithography machine with an exposure time of 330 milliseconds, a focal length range of -0.2 to 0.2, a light intensity of 650 to 750 mW / cm², a light intensity non-uniformity of less than 2% in the exposed area, and a minimum line width of 0.35 ± 0.05 micrometers (this is the purpose of exposing the photoresist film using a step-scan I-line lithography machine, i.e., the minimum line width of the photoresist film is 0.35 ± 0.05 micrometers).
[0054] (4) Spin wash the exposed wafer surface for 18 seconds, then spin the FHD-5 developer solution to cover all areas of the photoresist film surface, soak for 12 seconds, then spin at 250 rpm for 4 seconds to remove the developer solution, and then spin wash the wafer surface at 250 rpm for 18 seconds. The existing technology has a spin speed of 1500 rpm, which is one of the important reasons for photoresist strip bleed.
[0055] Steps (1) and (4) are repeated four times. In step (2), a thicker photoresist film is spin-coated, and in step (3), it is exposed according to the photolithographic pattern. In step (4), it is developed. The developer etches the exposed area much faster than the unexposed area, thus forming a photoresist strip in the unexposed area. In order to maintain the original thickness of the photoresist strip, the etching progress of the developer needs to be limited in step (4). That is, it is not necessary to etch the exposed area to the bottom all at once. If it is etched to the bottom all at once, the original thickness of the photoresist strip will also be greatly etched.
[0056] Therefore, step (1) needs to be performed again. The second HMDS film formed is uniform and continuous on the surface of the photoresist strip, relatively continuous on the sidewalls of the photoresist strip, but fragmented in the photoresist exposure area. Step (4) is performed again. On the one hand, the HMDS film in the exposure area is discontinuous, so the developer dissolves the photoresist still present in the exposure area more quickly. Conversely, due to the protection of the continuous HMDS film, the developer dissolves the upper surface and sidewalls of the photoresist strip much more slowly. On the other hand, the continuous HMDS film on the upper surface and sidewalls of the photoresist strip helps the photoresist strip resist water washing and immersion, and also provides mechanical reinforcement to prevent the photoresist from floating due to centrifugal force.
[0057] In this way, by repeating steps (1) and (4) four times, on the one hand, the exposure area is etched to the bottom through multiple developments, that is, etched to the wafer surface; on the other hand, the original thickness of the photoresist strip is preserved, that is, a larger aspect ratio of the photoresist strip is obtained.
[0058] The surface morphology of the photoresist obtained in preferred embodiment 1 is as follows: Figure 5 As shown, the cross-sectional morphology of the adhesive strip is as follows Figure 6 As shown.
[0059] Preferred embodiment 2
[0060] A method for improving photoresist bleaching during wafer development includes the following steps:
[0061] (1) Place the silicon carbide wafer in an oven at 130°C in an HMDS atmosphere for 130 seconds to form an HMDS film with a thickness of 30 nanometers on the wafer surface as a photoresist adhesive.
[0062] (2) Spin-coat an AZ MIR-703 photoresist film onto the HMDS film already formed on the wafer surface, and then dry and cure it; cure in an oven at 120°C for 120 seconds.
[0063] (3) The photoresist film is exposed using a step-scan I-line lithography machine. The exposure time is 360 milliseconds, the focal length range is -0.2 to 0.2, the light intensity is 650 to 750 mW / cm², the light intensity non-uniformity of the exposure area is less than 2%, and the narrowest line width of the photomask is 0.35 ± 0.05 micrometers.
[0064] (4) Spin wash the exposed wafer surface for 22 seconds, then spin the FHD-5 developer solution to cover all areas of the photoresist film surface, soak for 18 seconds, then spin at 350 rpm for 6 seconds to remove the developer solution, and then spin wash the wafer surface at 350 rpm for 22 seconds.
[0065] Repeat steps (1) and (4) three times.
[0066] The surface morphology and cross-sectional morphology of the photoresist obtained in preferred embodiment 2 are similar to those in preferred embodiment 1.
[0067] Preferred Example 3
[0068] A method for improving photoresist bleaching during wafer development includes the following steps:
[0069] (1) Place the silicon carbide wafer in an oven at 120°C in an HMDS atmosphere for 120 seconds to form an HMDS film with a thickness of 20 nanometers on the wafer surface as a photoresist adhesive.
[0070] (2) Spin-coat an AZ MIR-703 photoresist film onto the HMDS film already formed on the wafer surface, and then dry and cure it; cure in an oven at 120°C for 120 seconds.
[0071] (3) The photoresist film is exposed using a step-scan I-line lithography machine. The exposure time is 345 milliseconds, the focal length range is -0.2 to 0.2, the light intensity is 650 to 750 mW / cm², the light intensity non-uniformity of the exposure area is less than 2%, and the narrowest line width of the photomask is 0.35 ± 0.05 micrometers.
[0072] (4) Spin wash the exposed wafer surface for 20 seconds, then spin the FHD-5 developer solution to cover all areas of the photoresist film surface, soak for 15 seconds, then spin at 300 rpm for 5 seconds to remove the developer solution, and then spin wash the wafer surface at 300 rpm for 20 seconds.
[0073] Repeat steps (1) and (4) three times.
[0074] The cross-sectional morphology of the photoresist strip in preferred embodiment 3 is as follows: Figure 7 As shown.
[0075] Although the wafer material used in Examples 1-3 is silicon carbide, this should not be considered a limitation of the present invention, and the method of the present invention can still be applied to other semiconductor materials.
[0076] To test the development process effect of the method of the present invention, surface inspection by optical microscope (OEM) and cross-sectional inspection by SEM were performed. The inspection results and comparisons are as follows:
[0077] The minimum line width is 0.35±0.05 micrometers, the adhesive thickness is 1.8±0.1 micrometers, and the aspect ratio ranges from 4.2 to 6.2.
[0078] Traditional methods involve a single 60-second development cycle after exposure, at a speed of 1500 rpm, which results in bleaching after development. Figure 2 As shown, some adhesive strips are broken, and adjacent strips are bonded together, all due to adhesive drift. The surface morphology of the inclined adhesive strips is as follows. Figure 3 As shown, the adhesive strip twists under the centrifugal force of rotation, indicating a serious manufacturing defect. The morphology of the adhesive strip is observed in the SEM cross-section as follows: Figure 4 As shown, severe tilting has occurred, and for photoresist strips with a large aspect ratio, they may be flung off and break. The surface morphology of the photoresist after the process is improved using the method of this invention is as follows. Figure 5 The cross-sectional morphology of the rubber strip is as follows Figure 6 .
[0079] Using a more preferred embodiment of the present invention, the cross-sectional morphology of the adhesive strip with an aspect ratio of 5.3 obtained by testing shows that the adhesive strip remains straight and upright, and there are no problems of adhesive drift or tilting. Figure 7 As shown in the figure. However, in traditional processes, adhesive strips exhibit defects such as glue drift and tilting when the aspect ratio reaches 3.2. The test results and morphological comparisons demonstrate the superior process performance of this invention.
[0080] The embodiments of the present invention have been described in detail above with reference to the accompanying drawings. However, the present invention is not limited to the specific embodiments described above. The specific embodiments described above are merely illustrative and not restrictive. Those skilled in the art can make many modifications under the guidance of the present invention without departing from the spirit and scope of the claims. These modifications are all protected by the present invention.
Claims
1. A method for improving photoresist bleaching during wafer development, comprising the following steps: (1) Place the wafer in an oven with an HMDS atmosphere to form an HMDS film with a thickness of 5 to 30 nanometers on the wafer surface as a photoresist adhesive. (2) A photoresist film is spin-coated onto the HMDS adhesive film on the wafer, and then dried and cured; (3) Expose the photoresist film using a step-scan I-line lithography machine; (4) Rotate and wash the wafer surface, rotate and spread the developer solution to cover the photoresist film surface and immerse it, rotate and shake off the developer solution, and rotate and wash again. Repeat steps (1) and (4); In step (4): the exposed wafer surface is rotated and rinsed with water for 20±2 seconds, the developer is rotated and spread to all areas of the photoresist film surface, soaked for 15 to 20 seconds, the developer is shaken off by rotating at 300±50 rpm for 5±1 seconds, and then the wafer surface is rotated and rinsed with water for 20±2 seconds by rotating at 300±50 rpm.
2. The method of claim 1, wherein, In step (1): the temperature in the oven is 110-130℃ and the baking time is 110-130 seconds.
3. The method of claim 1, wherein, In step (1): the temperature in the oven is 120±1℃ and the baking time is 120 seconds.
4. The method of claim 1, wherein, In step (2), AZ MIR-703 photoresist is used, and the thickness of the photoresist film ranges from 1.8 to 2.1 micrometers.
5. The method of claim 1, wherein, In step (2), AZ MIR-6130 photoresist is used, and the thickness of the photoresist film ranges from 2.8 to 6 micrometers.
6. The method of claim 1, wherein, In step (3): the exposure time is 345±15 milliseconds, the focal length range is -0.2 to 0.2, the light intensity is 650 to 750 mW / cm², the light intensity non-uniformity of the exposure area is less than 2%, and the narrowest line width of the photomask is 0.35±0.05 micrometers.
7. The method of claim 6, wherein, The exposure time is 345 milliseconds.
8. The method of claim 6, wherein, In step (4): the exposed wafer surface is rotated and rinsed with water for 20 seconds, the developer is rotated and spread to all areas of the photoresist film surface, soaked for 15 seconds, then the developer is removed by rotating at 300 rpm for 5 seconds, and then the wafer surface is rotated and rinsed with water for 20 seconds by rotating at 300 rpm.
9. The method of claim 1, wherein, The thickness of the HMDS mucosa formed in step (1) is 10 to 20 nanometers.
10. The method according to any one of claims 1 to 9, wherein, Repeat steps (1) and (4) 2-4 times.
11. The method of claim 10, wherein, Repeat steps (1) and (4) three times.
Citation Information
Patent Citations
Photoetching method and device for oxide layer of silicon carbide diode
CN113433798A
Removal of alkaline crystal defects in lithographic patterning
US20130052593A1