Method and system for efficiently and selectively recovering iron phosphate product from sludge leachate
By adjusting the pH value of the sludge leaching liquid and adding iron salt, the efficient recovery of phosphorus elements in the sludge incineration ash is achieved, and the problem of impurities accompanied by dissolution in the existing technology is solved, the process flow is simplified and the recovery of iron phosphate is improved. Efficiency has significant economic advantages and application prospects.
Patent Information
- Application Number
- CN202310144580.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-02-21
AI Technical Summary
When recovering phosphorus elements from sludge incineration ash, the prior art has the problem of accompanying dissolution of impurity elements, which makes it difficult to recover high-purity phosphorus products, and the zirconium adsorbent process is complex and is not conducive to large-scale application.
By adjusting the pH value of the sludge leaching solution to acidity, adding iron salt and heating to 80°C, the phosphorus element is promoted to precipitate with iron phosphate hydrate, thereby achieving efficient recovery of iron phosphate products, simplifying the process flow and reducing costs.
The direct recycling of high-purity iron phosphate is achieved, the process flow is simplified, the cost is reduced, and the cumulative recycling efficiency of phosphorus elements is improved through recycling, reaching 81.1±1.8%, which has great economic advantages and market application prospects.
Smart Images

Figure CN116143094B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of phosphorus recovery, and more specifically, relates to a method and system for efficiently and selectively recovering iron phosphate products from sludge leachate. Background Art
[0002] At present, the global phosphorus mainly diffuses from high-concentration phosphate ore to low-concentration natural environment, resulting in the one-way flow and non-renewable characteristics of phosphorus in the biosphere. As an indispensable nutrient for plant growth, phosphorus is crucial to the development of modern agriculture. It is estimated that the global available phosphate reserves will be exhausted within 50-100 years. Therefore, it is necessary to find alternative resources for phosphate rock to meet the growing demand for phosphorus in modern agriculture.
[0003] A large amount of phosphorus consumed in daily production and life by humans enters the sewage treatment plant through the urban sewage pipe network. Among them, 90% of the phosphorus in the sewage is finally concentrated into the sludge through the biological phosphorus removal process or the chemical precipitation process. Therefore, municipal sludge contains a large amount of phosphorus. Municipal sludge, as a by-product of the sewage treatment process, needs to be properly treated and disposed. Sludge incineration technology, as a sludge harmless treatment technology, is a sludge treatment process promoted and applied in many countries. After municipal sludge is incinerated, the volume of sludge is greatly reduced, and the phosphorus in the sludge is further enriched. The phosphorus content is about 4.9-11.9wt%, which is equivalent to the phosphorus content in low-grade phosphate rock. At present, the annual output of sludge incineration ash in the world is about 1.7 million tons after incineration. The annual output of sludge incineration ash is huge and can be used as a substitute for phosphate rock to meet the growing demand for phosphorus. However, a large amount of other heavy metal elements are also enriched in the sludge incineration ash during the sludge incineration process, which increases the difficulty of recovering the phosphorus element in the sludge incineration ash. Therefore, it is necessary to develop various technologies to improve the purity of the recovered phosphorus products.
[0004] At present, wet extraction technology is the mainstream technology for recovering phosphorus from sludge incineration ash. This technology mainly uses acidic reagents such as organic acids and inorganic acids to dissolve phosphorus in sludge incineration ash into a solution, and then recovers phosphorus from the solution (leaching solution). In particular, the phosphorus in sludge incineration ash is dissolved into a solution using H2SO4 solution, and the phosphorus leaching efficiency is as high as 90-100%. However, during the acid leaching process, other soluble elements and heavy metal elements in sludge incineration ash are inevitably dissolved into the leachate, which greatly increases the difficulty of recovering high-purity phosphorus products from the leachate.
[0005] The researchers found that the concentration of cationic impurities in the leachate can be reduced by ion exchange through cation exchange resin, and then NH4 is added in a strict molar ratio. + and Mg 2+, and strictly control the pH of the leachate to produce high-purity struvite products. Multiple extraction technology can reduce the concentration of impurity ions in the leachate through multiple extractions, thereby increasing the concentration of subsequent phosphorus products. First, the impurity elements in the sludge incineration ash are extracted with ethylenediaminetetraacetic acid solution, and then the sludge incineration ash from which the impurity elements have been extracted is leached again with H2SO4 solution to reduce the impurity elements in the leachate, and finally quicklime is added to produce high-purity calcium-phosphorus products. However, the phosphorus products produced by these two technologies require additional purification treatment to achieve the recovery of high-purity phosphorus products, and the phosphorus product recovery process is complicated and expensive.
[0006] Researchers have found that adsorbents prepared based on zirconium have specific adsorption for phosphorus and can selectively recover phosphorus directly from sludge leachate without any purification process. However, the process of recovering phosphorus products using zirconium adsorbent technology is complicated, including a series of processes such as the adsorption-desorption process of phosphorus and the production of phosphorus products. In addition, the preparation process of zirconium adsorbents is complicated, and the subsequent reduction in the adsorption capacity of zirconium adsorbents requires the adsorbent to be treated and disposed of, which is not conducive to large-scale application. Therefore, it is necessary to develop a technology for efficient recovery of phosphorus that is simple to operate, has mild operating conditions, and has low economic costs. Summary of the invention
[0007] In order to solve the deficiencies in the prior art, the present invention provides a method for directly and efficiently selectively recovering phosphorus from sludge leachate. The method does not require additional purification pretreatment, only requires adding a certain amount of iron to the leachate, slightly adjusting the pH of the leachate to about 1.2, and precipitating iron phosphate hydrate in a water bath at 80°C for 30 minutes, thereby achieving efficient recovery of phosphorus in sludge incineration ash. The method is simple and easy to operate, and has great economic advantages and application prospects.
[0008] The present invention adopts the following technical solution.
[0009] The method for efficiently and selectively recovering iron phosphate product from sludge leachate comprises the following steps:
[0010] The pH value of the sludge leaching solution containing phosphorus is adjusted to be acidic, the leaching solution is heated, iron salt is added, the phosphorus element in the leaching solution is precipitated in the form of iron phosphate hydrate, and the iron phosphate hydrate precipitate is recovered.
[0011] Preferably, the pH value of the phosphorus-containing sludge leachate is adjusted to between 1 and 2, the leachate is heated, the temperature of the leachate is controlled to be within a set temperature range and kept warm, iron salt is added based on the molar amount of phosphorus, the phosphorus in the leachate is precipitated in the form of iron phosphate hydrate, and solid-liquid separation is performed to obtain the iron phosphate hydrate precipitate and the leachate.
[0012] Preferably, sludge incineration ash is added to the leachate after separation of the ferric phosphate hydrate precipitate, and the leachate is recycled.
[0013] Preferably, the method specifically comprises the following steps:
[0014] Step 1: putting the sludge incineration ash into H2SO4 solution to obtain sludge leaching solution rich in phosphorus;
[0015] Step 2: The sludge leachate obtained in step 1 is separated into solid and liquid to obtain residue and leachate, iron salt is added to the leachate, acid and alkali solution is added to adjust the pH of the leachate to a set range, the temperature of the leachate is controlled to a set range, and the iron phosphate hydrate precipitate is recovered.
[0016] Preferably, step 1 comprises:
[0017] Step 1.1: Incinerate municipal sewage sludge in an incinerator to obtain sewage sludge incineration ash;
[0018] Step 1.2: Add the sludge incineration ash into 0.2 mol / L H2SO4 solution at a liquid-to-solid ratio of 50 mL / g, and record the solution pH as the initial pH;
[0019] Step 1.3: The H2SO4 solution mixed with the sludge incineration ash is oscillated and leached at 200 rpm in an oscillating incubator for 12 hours, so that the phosphorus element in the sludge incineration ash is fully acid-dissolved into the solution to obtain a sludge leachate rich in phosphorus element.
[0020] Preferably, step 2 comprises:
[0021] Step 2.1: separating the sludge leachate into solid and liquid to obtain residue and leachate;
[0022] Step 2.2: measuring the phosphorus concentration in the leachate, and adding iron at a stoichiometric molar ratio of 1:1 based on the molarity of phosphorus;
[0023] Step 2.3: Add acid and alkali solution to adjust the pH of the leachate to the target pH value of 1.2, control the temperature of the leachate to 80°C and keep it warm for 30 minutes to promote the precipitation of phosphorus in the leachate in the form of iron phosphate hydrate:
[0024] Step 2.4: solid-liquid separation to obtain iron phosphate hydrate precipitate and leachate;
[0025] Step 2.5: The iron phosphate hydrate precipitate is placed in an oven and dried at 70° C. for 10 h to obtain a dry iron phosphate hydrate precipitate.
[0026] Preferably, the process further comprises step 3: recycling the leaching solution obtained after separating the iron phosphate hydrate precipitate in step 2, specifically comprising:
[0027] The pH value of the leachate after separating the ferric phosphate hydrate precipitate in step 2 is adjusted to the initial pH, and sludge incineration ash is added. The acid dissolution process of phosphorus in the sludge incineration ash is consistent with step 1, and then an amount of iron element equal to that in step 2 is added to the leachate, and the recovery process of the phosphorus product in the sludge leachate is consistent with step 2.
[0028] Preferably, the method further comprises step 4: after the phosphorus element in the leachate of step 3 is initially precipitated as ferric phosphate hydrate, the leachate after the initial precipitation is again water-bathed to recover the phosphorus element in the form of ferric phosphate hydrate.
[0029] Preferably, the method further comprises step 5: recycling the leachate in step 4 for a third time after separating the ferric phosphate hydrate precipitate; during the third recycling of the leachate, the phosphorus recovery process in the sludge incineration ash is consistent with the phosphorus recovery process in the second recycling of the sludge leachate, and the specific recovery steps are consistent with steps 3 and 4 in sequence;
[0030] Step 6: the leachate in step 5 is recycled for the fourth time after the iron phosphate hydrate precipitate is separated; during the fourth recycling of the leachate, the recovery step of phosphorus in the sludge incineration ash is the same as step 5;
[0031] Step 7: the ferric phosphate hydrate precipitate is separated twice from the leachate in step 6 and then recycled for the fifth time; during the fifth recycling of the leachate, after the phosphorus element in the sludge incineration ash is released into the leachate, the phosphorus element in the leachate needs to be recovered in the form of ferric phosphate hydrate precipitate through three precipitations; the first two recovery steps of the phosphorus element in the leachate are consistent with step 6, and the third recovery step of the phosphorus element in the leachate is consistent with the second recovery step.
[0032] A system for efficiently and selectively recovering iron phosphate products from sludge leachate includes a pH adjustment module, a temperature control module, an iron element addition module and a recovery module, which are respectively used to adjust the pH value of the sludge leachate containing phosphorus elements to acidic, heat the leachate, add iron salt, precipitate the phosphorus elements in the leachate in the form of iron phosphate hydrate, and then recover the iron phosphate hydrate precipitate.
[0033] The beneficial effect of the present invention is that, compared with the prior art, the present invention proposes a method and system for efficiently recovering phosphorus directly from sludge leachate, and proposes for the first time that phosphorus in sludge leachate can be directly recovered from sludge leachate in the form of high-purity iron phosphate hydrate by precipitation only by adjusting pH, adding iron salt and controlling temperature without purification pretreatment. Specifically:
[0034] (1) The present invention mainly promotes the production of high-purity iron phosphate products by adding an iron dosage to the leachate and controlling the pH and temperature of the leachate. The method needs to add a certain amount of iron element to the leachate to produce phosphorus products. Iron element is widely distributed on the earth, cheap and easy to obtain, which is conducive to the large-scale application of the method.
[0035] (2) The initial sludge leachate after acid leaching is acidic in nature, and only a slight adjustment of the pH is required to achieve the target pH value of the sludge leachate. Therefore, the dosage of acid and alkali reagents required to adjust the sludge leachate is relatively small.
[0036] (3) The present invention needs to control the temperature of the leaching solution to 80°C and maintain it for 30 minutes, thereby promoting the production of iron phosphate. The electric energy required to control the temperature of the leaching solution can be supplied by electric energy generated by green energy such as solar energy and wind energy, and can be carried out at night when the load on the power grid is low, so the cost of the electric energy required by this method is also economical.
[0037] (4) After the phosphorus product is initially recovered from the leachate by the present invention, the sludge leachate is still acidic and can be used as the initial acidic solution for leaching phosphorus from the sludge incineration ash next time, thereby realizing the recycling of the acidic leachate ( Figure 1 ). During the recycling process of the acidic leaching solution, the efficiency of phosphorus recovery from the sludge leaching solution gradually increased, and the purity of the recovered phosphorus product was still high. After the sludge leaching solution was recycled for 5 times, the cumulative recovery efficiency of phosphorus in the sludge leaching solution was as high as 81.1±1.8% ( Figure 2 ), the recovered phosphorus product mainly exists in the form of iron phosphate hydrate ( Figure 3 ).
[0038] Therefore, compared with other methods for recovering phosphorus from sludge incineration ash, the present invention is not only simple to operate, has mild operating conditions, and requires cheap and readily available reagents, but also has higher efficiency and purity in recovering phosphorus from sludge recovery ash, and has relatively large economic advantages and market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 The present invention is a flow chart of a method for efficiently and selectively recovering iron phosphate products from sludge leachate;
[0040] Figure 2 is the cumulative recovery efficiency of phosphorus from sludge incineration ash in the present invention;
[0041] Figure 3 The present invention discloses a phase composition of the phosphorus product recovered from sludge incineration ash after calcination. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The embodiments described in this application are only part of the embodiments of the present invention, not all of them. Based on the spirit of the present invention, other embodiments obtained by ordinary technicians in this field without creative work are all within the scope of protection of the present invention.
[0043] like Figure 1 As shown, an embodiment of the present invention provides a method for efficiently and selectively recovering an iron phosphate product from a sludge leachate, comprising the following steps:
[0044] The pH value of the sludge leaching solution containing phosphorus is adjusted to be acidic, the leaching solution is heated, iron salt is added, the phosphorus element in the leaching solution is precipitated in the form of iron phosphate hydrate, and the iron phosphate hydrate precipitate is recovered.
[0045] In a preferred but non-limiting embodiment of the present invention, the method for efficiently and selectively recovering the iron phosphate product from the sludge leachate specifically comprises the following steps:
[0046] The pH value of the phosphorus-containing sludge leachate is adjusted to between 1 and 2, with a more preferred pH value of 1.2, the leachate is heated, the leachate temperature is controlled to be within a set temperature range and kept warm, iron salt is added based on the molar amount of phosphorus, the phosphorus in the leachate is precipitated in the form of iron phosphate hydrate, and the iron phosphate hydrate precipitate and the leachate are obtained by solid-liquid separation, thereby realizing the recovery of phosphorus in sludge incineration ash.
[0047] In a further preferred but non-limiting embodiment of the present invention, the method for efficiently and selectively recovering the iron phosphate product from the sludge leachate more specifically comprises the following steps:
[0048] The pH value of the phosphorus-containing sludge leachate is adjusted to between 1 and 2, the leachate is heated to control the leachate temperature to above 60°C, preferably 80°C and kept warm, iron salt is added based on the mole of phosphorus element, so that the phosphorus element in the leachate is precipitated in the form of iron phosphate hydrate, solid-liquid separation is performed to obtain the iron phosphate hydrate precipitate and the leachate, phosphorus element in the sludge incineration ash is recovered, sludge incineration ash is added to the leachate after separating the iron phosphate hydrate precipitate, acid and alkali solution is added to adjust the pH value, and the leachate is recycled.
[0049] In a further preferred but non-limiting embodiment of the present invention, the method for efficiently and selectively recovering the iron phosphate product from the sludge leachate more specifically comprises the following steps:
[0050] Step 1: Put the sludge incineration ash into H2SO4 solution to obtain sludge leaching solution rich in phosphorus.
[0051] Preferably, step 1 specifically includes:
[0052] Step 1.1: The municipal sludge in the sewage treatment plant is incinerated in an incinerator at 850°C to obtain sludge incineration ash;
[0053] Step 1.2: Add the sludge incineration ash into a 0.2 mol / L H2SO4 solution at a liquid-to-solid ratio of 50 mL / g, and record the pH of the solution at this time as the initial pH;
[0054] Step 1.3: The H2SO4 solution mixed with the sludge incineration ash is then leached in an oscillating incubator at 200 rpm for 12 hours, so that the phosphorus element in the sludge incineration ash is fully acid-dissolved into the solution to obtain a sludge leachate rich in phosphorus element.
[0055] Step 2: The sludge leachate obtained in step 1 is separated into solid and liquid to obtain residue and leachate, iron salt is added to the leachate, acid and alkali solution is added to adjust the pH of the leachate to a set range, the temperature of the leachate is controlled to a set range, and the iron phosphate hydrate precipitate is recovered.
[0056] Preferably, step 2 specifically includes:
[0057] Step 2.1: separating the sludge leachate into solid and liquid to obtain residue and leachate;
[0058] Step 2.2: Then measure the phosphorus concentration in the leachate, and add iron at a stoichiometric molar ratio of about 1:1 based on the molar ratio of phosphorus; that is, the amount of iron salt added is about the iron-phosphorus molar ratio of about 1:1, which is not strictly required to be 1:1, and the preferred molar ratio is 1:1. This method emphasizes the addition of a certain amount of iron salt to generate iron phosphate.
[0059] Step 2.3: Add acid and alkali solution to adjust the pH of the leachate to the target pH value, preferably 1.2, control the temperature of the leachate to 80°C and keep it warm for 30 minutes to promote the precipitation of phosphorus in the leachate in the form of iron phosphate hydrate:
[0060] Step 2.4: Then, solid-liquid separation is performed to obtain iron phosphate hydrate precipitate and leaching solution, thereby realizing the recovery of phosphorus in the sludge incineration ash;
[0061] Step 2.5: Place the iron phosphate hydrate precipitate in an oven and dry it at 70° C. for 10 h to obtain a dry iron phosphate hydrate precipitate for easy storage.
[0062] It is understandable that even if the precipitate is dried in an oven at 70°C for 10 hours, what is obtained is ferric phosphate hydrate. What is removed in the oven is the water attached to the surface of the precipitate. At this time, the water in the ferric phosphate hydrate exists in the form of bound water. The bound water can be further removed after calcination at 720°C.
[0063] Step 1 and step 2 are Figure 1 The flow chart shows the specific operation process of phosphorus product recovery when the sludge leachate is recycled for the first time.
[0064] Step 3: The pH of the leachate after the ferric phosphate hydrate precipitate is separated in step 2 is about 1.2, and the leachate contains a large amount of hydrogen ions. In order to save acid reagents, the leachate is recycled for the second time. The pH value of the leachate after the ferric phosphate hydrate precipitate is separated in step 2 is adjusted, and sludge incineration ash is added. The acid dissolution process of phosphorus in the sludge incineration ash is the same as step 1, and then the same amount of iron as step 2 is added to the leachate. The recovery process of phosphorus products in the sludge leachate is the same as step 2, and the second recycling of the leachate is completed.
[0065] Preferably, step 3 specifically includes:
[0066] Step 3.1: adding a small amount of H2SO4 reagent to the leachate after the iron phosphate hydrate precipitate is separated in step 2, and adjusting the pH of the leachate to be consistent with the initial pH in step 1;
[0067] Step 3.2: adding the sludge incineration ash to the leaching solution at a liquid-solid ratio of 50 mL / g, and the acid dissolution process of phosphorus in the sludge incineration ash is the same as step 1;
[0068] Step 3.3: Add an amount of iron element equal to that in step 2 to the leachate. The recovery process of the phosphorus product in the sludge leachate is the same as that in step 2.
[0069] Step 4: After the phosphorus in the leachate in step 3 is initially precipitated as ferric phosphate hydrate, the leachate still contains a large amount of phosphorus and iron. In order to improve the recovery efficiency of phosphorus, the leachate after the initial precipitation needs to be water-bathed again and phosphorus is recovered in the form of ferric phosphate hydrate.
[0070] Preferably, step 4 specifically comprises: in step 3, after the initial precipitation of iron phosphate hydrate in the leachate, solid-liquid separation is performed to obtain iron phosphate hydrate precipitation and leachate, and then, without adding iron element, the leachate temperature is controlled at 80° C. and kept warm for 30 minutes to promote the generation of iron phosphate hydrate precipitation again, thereby improving the recovery efficiency of phosphorus in the leachate during the second recycling of the leachate.
[0071] Steps 3 and 4 are Figure 1 The flow chart shows the specific operation process of phosphorus product recovery when the sludge leachate is recycled for the second time.
[0072] Step 5: After separating the iron phosphate hydrate precipitate, the leachate in step 4 is recycled for a third time. During the third recycling of the leachate, the phosphorus recovery process in the sludge incineration ash is consistent with the phosphorus recovery process during the second recycling of the sludge leachate, and the specific recovery steps are consistent with steps 3 and 4.
[0073] Step 6: After separating the iron phosphate hydrate precipitate from the leachate in step 5, the fourth recycling step is performed. During the fourth recycling process of the leachate, the recovery step of phosphorus in the sludge incineration ash is the same as step 5. Steps 5 and 6 are Figure 1 The specific operation process of phosphorus product recovery process when the sludge leachate is recycled for the third and fourth time in the flow chart.
[0074] Step 7: Separate the ferric phosphate hydrate precipitate from the leachate in step 6 twice and then recycle it for the fifth time. During the fifth recycling of the leachate, after the phosphorus in the sludge incineration ash is released into the leachate, the phosphorus in the leachate needs to be recovered in the form of ferric phosphate hydrate precipitate through three precipitations. The first two recovery steps of the phosphorus in the leachate are consistent with step 6, and the third recovery step of the phosphorus in the leachate is consistent with the second recovery step. Step 7 is Figure 1 The specific operation process of phosphorus product recovery during the fifth recycling of sludge leachate in the flow chart.
[0075] It is worth noting that in a preferred embodiment of the present invention, five cycles of utilization are a preferred but non-limiting implementation means, such as Figure 2 As shown, after only one implementation, the recovery efficiency of the present invention has reached about 55.0±2.2%, and multiple recycling can improve the cumulative recovery efficiency. In other words, in order to achieve the set cumulative recovery efficiency, those skilled in the art can make a trade-off between the number of recycling times, and any number of cycles falls within the core concept of the present invention.
[0076] It is also worth noting that when recovering iron phosphate from the sludge leachate, the leachate is heated, the pH is between 1-2, and iron salt is added to recover a certain amount of iron phosphate. The seven steps of phosphorus recovery in the specific implementation are the specific operating conditions for the present invention to be optimized. The core concept of the present invention is that the leachate is heated, the pH of the leachate is adjusted, and iron salt is added to the leachate. The above conditions are met and then the iron phosphate hydrate precipitate is recovered from the sludge leachate, which is within the scope of protection of the present invention.
[0077] The embodiment of the present invention also provides a system for efficiently and selectively recovering an iron phosphate product from a sludge leachate, comprising a pH adjustment module, a temperature control module, an iron element addition module and a recovery module, which are respectively used to adjust the pH value of the phosphorus-containing sludge leachate to be acidic, heat the leachate, add iron salt, precipitate the phosphorus element in the leachate in the form of iron phosphate hydrate, and then recover the iron phosphate hydrate precipitate.
[0078] The beneficial effect of the present invention is that, compared with the prior art, the method mainly promotes the production of high-purity iron phosphate products by adding an iron dosage to the leachate and controlling the pH and temperature of the leachate. The method needs to add a certain amount of iron element to the leachate to produce phosphorus products, and iron element is widely distributed on the earth, cheap and easy to obtain, which is conducive to the large-scale application of the method. The initial sludge leachate after acid leaching itself is acidic, and only a slight adjustment of the pH is required to achieve a pH of about 1.2 in the sludge leachate, so the dosage of acid and alkali reagents required to adjust the sludge leachate is less. The method needs to control the temperature of the leachate to 80°C and maintain it for 30 minutes, thereby promoting the production of iron phosphate. The electric energy required to control the temperature of the leachate can be supplied by electric energy generated by green energy such as solar energy and wind energy, and can be carried out at night when the grid load is low, so the cost of the electric energy required for the method is also economical. After the phosphorus product is initially recovered from the leaching solution by this method, the sludge leaching solution is still acidic and can be used as the initial acid solution for leaching phosphorus from the sludge incineration ash next time, thereby realizing the recycling of the acidic leaching solution ( Figure 1 ). During the recycling process of the acidic leaching solution, the efficiency of phosphorus recovery from the sludge leaching solution gradually increased, and the purity of the recovered phosphorus product was still high. After the sludge leaching solution was recycled for 5 times, the cumulative recovery efficiency of phosphorus in the sludge leaching solution was as high as 81.1±1.8% ( Figure 2 ), the recovered phosphorus product mainly exists in the form of iron phosphate hydrate, and after calcination to remove water, the precipitate is mainly iron phosphate ( Figure 3 ). Therefore, compared with other methods for recovering phosphorus from sludge incineration ash, this method is not only simple to operate, has mild operating conditions, and requires cheap and readily available reagents, but also has high efficiency and purity in recovering phosphorus from sludge recovery ash, and has relatively large economic advantages and market application prospects.
[0079] The present disclosure may be a system, a method and / or a computer program product. The computer program product may include a computer-readable storage medium carrying computer-readable program instructions for causing a processor to implement various aspects of the present disclosure.
[0080] A computer-readable storage medium may be a tangible device that can hold and store instructions used by an instruction execution device. A computer-readable storage medium may be, for example, but not limited to, an electrical storage device, a magnetic storage device, an optical storage device, an electromagnetic storage device, a semiconductor storage device, or any suitable combination of the foregoing. More specific examples of computer-readable storage media (a non-exhaustive list) include: a portable computer disk, a hard disk, a random access memory (RAM), a read-only memory (ROM), an erasable programmable read-only memory (EPROM or flash memory), a static random access memory (SRAM), a portable compact disk read-only memory (CD-ROM), a digital versatile disk (DVD), a memory stick, a floppy disk, a mechanical encoding device, such as a punch card or a raised structure in a groove on which instructions are stored, and any suitable combination of the foregoing. As used herein, a computer-readable storage medium is not to be interpreted as a transient signal per se, such as a radio wave or other freely propagating electromagnetic wave, an electromagnetic wave propagating through a waveguide or other transmission medium (e.g., a light pulse through a fiber optic cable), or an electrical signal transmitted through a wire.
[0081] The computer-readable program instructions described herein can be downloaded from a computer-readable storage medium to each computing / processing device, or downloaded to an external computer or external storage device via a network, such as the Internet, a local area network, a wide area network, and / or a wireless network. The network can include copper transmission cables, optical fiber transmissions, wireless transmissions, routers, firewalls, switches, gateway computers, and / or edge servers. The network adapter card or network interface in each computing / processing device receives the computer-readable program instructions from the network and forwards the computer-readable program instructions for storage in the computer-readable storage medium in each computing / processing device.
[0082] The computer program instructions for performing the operation of the present disclosure may be assembly instructions, instruction set architecture (ISA) instructions, machine instructions, machine-related instructions, microcode, firmware instructions, state setting data, or source code or object code written in any combination of one or more programming languages, including object-oriented programming languages, such as Smalltalk, C++, etc., and conventional procedural programming languages, such as "C" language or similar programming languages. Computer-readable program instructions may be executed completely on a user's computer, partially on a user's computer, as an independent software package, partially on a user's computer, partially on a remote computer, or completely on a remote computer or server. In the case of a remote computer, the remote computer may be connected to the user's computer via any type of network, including a local area network (LAN) or a wide area network (WAN), or may be connected to an external computer (e.g., using an Internet service provider to connect via the Internet). In some embodiments, an electronic circuit, such as a programmable logic circuit, a field programmable gate array (FPGA), or a programmable logic array (PLA), may be customized by utilizing the state information of the computer-readable program instructions, and the electronic circuit may execute the computer-readable program instructions, thereby realizing various aspects of the present disclosure.
[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents, and any modifications or equivalent replacements that do not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A method for efficiently and selectively recovering iron phosphate products from sludge leachate, characterized in that: The following steps are involved: The pH value of the phosphorus-containing sludge leachate is adjusted to between 1 and 2, the leachate is heated, the leachate temperature is controlled to be 80°C and kept warm, iron salt is added, and iron is added at a stoichiometric molar ratio of 1:1 based on the mole of phosphorus, the phosphorus in the leachate is precipitated in the form of iron phosphate hydrate, and the iron phosphate hydrate precipitate is recovered.
2. The method for efficiently and selectively recovering iron phosphate products from sludge leachate according to claim 1, characterized in that: The pH value of the sludge leachate containing phosphorus is adjusted to between 1 and 2, the leachate is heated, the temperature of the leachate is controlled to be within a set temperature range and kept warm, iron salt is added based on the mole of phosphorus element, the phosphorus element in the leachate is precipitated in the form of iron phosphate hydrate, and solid-liquid separation is performed to obtain the iron phosphate hydrate precipitate and the leachate.
3. The method for efficiently and selectively recovering ferric phosphate products from sludge leachate according to claim 2, characterized in that: Sludge incineration ash is added to the leachate after separation of iron phosphate hydrate precipitation, and the leachate is recycled.
4. The method for efficiently and selectively recovering ferric phosphate products from sludge leachate according to claim 1, characterized in that: The specific steps include: Step 1: putting the sludge incineration ash into H2SO4 solution to obtain sludge leaching solution rich in phosphorus; Step 2: The sludge leachate obtained in step 1 is separated into solid and liquid to obtain residue and leachate, iron salt is added to the leachate, acid and alkali solution is added to adjust the pH of the leachate to a set range, the temperature of the leachate is controlled to a set range, and the iron phosphate hydrate precipitate is recovered.
5. The method for efficiently and selectively recovering iron phosphate products from sludge leachate according to claim 1, characterized in that: Step 1 includes: Step 1.1: Incinerate municipal sewage sludge in an incinerator to obtain sewage sludge incineration ash; Step 1.2: Add the sludge incineration ash into 0.2 mol / L H2SO4 solution at a liquid-to-solid ratio of 50 mL / g, and record the solution pH as the initial pH; Step 1.3: The H2SO4 solution mixed with the sludge incineration ash is oscillated and leached at 200 rpm in an oscillating incubator for 12 hours, so that the phosphorus element in the sludge incineration ash is fully acid-dissolved into the solution to obtain a sludge leachate rich in phosphorus element.
6. The method for efficiently and selectively recovering iron phosphate products from sludge leachate according to claim 5, characterized in that: Step 2 includes: Step 2.1: separating the sludge leachate into solid and liquid to obtain residue and leachate; Step 2.2: measuring the phosphorus concentration in the leachate, and adding iron at a stoichiometric molar ratio of 1:1 based on the molarity of phosphorus; Step 2.3: Add acid and alkali solution to adjust the pH of the leachate to the target pH value of 1.2, control the temperature of the leachate to 80°C and keep it warm for 30 minutes to promote the precipitation of phosphorus in the leachate in the form of iron phosphate hydrate: Step 2.4: solid-liquid separation to obtain iron phosphate hydrate precipitate and leachate; Step 2.5: The iron phosphate hydrate precipitate is placed in an oven and dried at 70° C. for 10 h to obtain a dry iron phosphate hydrate precipitate.
7. The method for efficiently and selectively recovering ferric phosphate products from sludge leachate according to claim 5 or 6, characterized in that: The step 3 is also included: recycling the leaching solution obtained after the iron phosphate hydrate precipitate separated in the step 2, specifically: The pH value of the leachate after separating the ferric phosphate hydrate precipitate in step 2 is adjusted to the initial pH, and sludge incineration ash is added. The acid dissolution process of phosphorus in the sludge incineration ash is consistent with step 1, and then an amount of iron element equal to that in step 2 is added to the leachate, and the recovery process of the phosphorus product in the sludge leachate is consistent with step 2.
8. The method for efficiently and selectively recovering ferric phosphate products from sludge leachate according to claim 7, characterized in that: The step 4 is also included: after the phosphorus element in the leachate in step 3 is initially precipitated as ferric phosphate hydrate, the leachate after the initial precipitation is again water-bathed to recover the phosphorus element in the form of ferric phosphate hydrate.
9. The method for efficiently and selectively recovering ferric phosphate products from sludge leachate according to claim 8, characterized in that: The invention also includes step 5: recycling the leachate in step 4 for a third time after separating the iron phosphate hydrate precipitate; during the third recycling of the leachate, the phosphorus recovery process in the sludge incineration ash is consistent with the phosphorus recovery process in the second recycling of the sludge leachate, and the specific recovery steps are consistent with steps 3 and 4 in sequence; Step 6: the leachate in step 5 is recycled for the fourth time after the iron phosphate hydrate precipitate is separated; during the fourth recycling of the leachate, the recovery step of phosphorus in the sludge incineration ash is the same as step 5; Step 7: the ferric phosphate hydrate precipitate is separated twice from the leachate in step 6 and then recycled for the fifth time; during the fifth recycling of the leachate, after the phosphorus element in the sludge incineration ash is released into the leachate, the phosphorus element in the leachate needs to be recovered in the form of ferric phosphate hydrate precipitate through three precipitations; the first two recovery steps of the phosphorus element in the leachate are consistent with step 6, and the third recovery step of the phosphorus element in the leachate is consistent with the second recovery step.
10. A system for efficiently and selectively recovering iron phosphate products from sludge leachate, for implementing the method according to any one of claims 1 to 9, characterized in that: The method comprises a pH value adjustment module, a temperature control module, an iron element addition module and a recovery module, which are respectively used for adjusting the pH value of the phosphorus-containing sludge leaching solution to be acidic, heating the leaching solution, adding iron salt, precipitating the phosphorus element in the leaching solution in the form of iron phosphate hydrate, and then recovering the iron phosphate hydrate precipitate.