A method for resource disposal of environmentally friendly slag containing beryllium and its application
By roasting the beryllium-containing environmentally friendly slag with high fixed carbon content, the coal auxiliary materials for reducing the content of high carbon, the cured beryllium silicate is solved, and the problems of environmental pollution and high cost in the existing technology are achieved, and safe and efficient environmentally friendly slag disposal and resources are achieved. utilizing.
Patent Information
- Application Number
- CN202310071968.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-02-07
AI Technical Summary
The existing technology lacks effective methods to safely and economically dispose of beryllium-containing environmentally friendly slag, which leads to environmental pollution, and the existing processes are complex and costly, which affects the resource utilization of environmentally friendly slag.
Mix beryllium-containing environmentally friendly slag with high fixed carbon content and roast at 850℃ to 1000℃. The beryllium sulfate is decomposed through a reducing atmosphere to reduce the sulfur content, form cured beryllium silicate, and reduce toxic beryllium leaching. It is suitable for Mixed material in cement clinker.
It realizes low-cost and low-energy-consuming roasting treatment, reduces the toxic beryllium leaching content, and the product can be used in cement clinker, reduces environmental pollution, and meets the requirements of safety, efficiency and green disposal.
Smart Images

Figure BDA0004065000100000071
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid waste disposal, and in particular relates to a resource disposal method and application of beryllium-containing environmentally friendly slag. Background Art
[0002] Beryllium and its alloys are irreplaceable strategic metal materials in the fields of aviation, aerospace, military industry, electronics, nuclear energy, etc. At present, the sulfuric acid method is mainly used to produce beryllium oxide. A certain amount of beryllium-containing waste slag is produced during the production process. According to different slag production links, there are mainly four types of beryllium-containing environmentally friendly slag, silicon slag, iron slag, and aluminum ammonium alum slag. Among them, beryllium-containing environmentally friendly slag is the precipitated slag formed by the treatment of beryllium-containing wastewater produced in the production process of beryllium oxide with lime milk. Beryllium is a toxic element to humans and animals. If it is not safely disposed of, it will threaten the ecological environment. At present, there is a lack of technical support for the disposal of beryllium-containing environmentally friendly slag, and there is a blank in the research of related disposal technologies at home and abroad. Therefore, it is of great significance to carry out research on the harmless technology of resource utilization of beryllium-containing environmentally friendly slag, solve the storage problem of beryllium-containing environmentally friendly slag, realize the safe and efficient disposal of beryllium-containing environmentally friendly slag, and provide technical support for the safe disposal of beryllium-containing environmentally friendly slag nationwide, and at the same time escort the sustainable development of the military products industry.
[0003] Chinese invention patent CN109761514B discloses a beryllium slag detoxification and cement kiln coordinated resource processing system and process, which washes the beryllium slag under acidic conditions, obtains beryllium sulfate solution to recover beryllium hydroxide, and the obtained solid slag enters the cement kiln for high-temperature calcination to make cement raw materials. The process is complicated and has high operating costs. Chinese invention patent CN109706327B discloses a method for harmless disposal of beryllium slag, which uses beryllium slag as a slag-type auxiliary material for blast furnace lead smelting, enters the blast furnace for smelting, and obtains harmless molten slag. The smelting temperature of this process is relatively high, and the quality of crude lead alloy products is easily affected. Summary of the invention
[0004] In order to overcome the technical problem of environmental pollution caused by the storage of beryllium-containing environmentally friendly slag in the prior art, the present invention provides a resource disposal method and application of beryllium-containing environmentally friendly slag, which has a simple disposal process, low equipment investment, low operating cost, good solidification effect of roasting products, no generation of three wastes, and low environmental pollution, meeting the requirements of safe, efficient and green disposal of beryllium-containing environmentally friendly slag.
[0005] In order to solve the above technical problems, the technical solutions proposed by the present invention are as follows:
[0006] The first aspect of the present invention provides a method for recycling beryllium-containing environmentally friendly slag, comprising the following steps:
[0007] S1. Evenly mix the beryllium-containing environmentally friendly slag and auxiliary materials to obtain the beryllium-containing environmentally friendly slag with auxiliary materials, wherein the auxiliary materials are added in an amount of 2-10% of the mass of the beryllium-containing environmentally friendly slag.
[0008] The auxiliary material is a kind of reducing coal, wherein the fixed carbon content is greater than 55% and the calorific value is greater than 4000 kcal / kg.
[0009] S2. The beryllium-containing environmentally friendly slag mixed in S1 is roasted at 850° C. to 1000° C. to obtain a roasted sample.
[0010] In the present invention, the roasting temperature of the beryllium-containing environmentally friendly slag and auxiliary materials is set to 850°C-1000°C. If the roasting temperature is lower than 850°C, the reaction will be insufficient and the beryllium solidification effect will not meet the toxicity leaching requirements; if the roasting temperature is higher than 1000°C, sintering will occur and energy consumption will increase.
[0011] As an optional implementation, in the resource recovery method provided by the present invention, the roasting temperature is 900°C to 1000°C.
[0012] The auxiliary material in the present invention is a kind of reducing coal, wherein the fixed carbon content is greater than 55% and the calorific value is greater than 4000kcal / kg. The auxiliary material in the present invention is a substance that changes the reaction mode, improves the efficiency of beryllium fixation, reduces the temperature of beryllium fixation, and improves the sulfate desulfurization rate. The auxiliary material is added to the beryllium-containing environmental slag for roasting treatment. The C in the auxiliary material allows the roasting to be carried out in a reducing atmosphere. The reducing atmosphere is conducive to the decomposition of beryllium sulfate and other sulfates, and reduces the reaction temperature of beryllium sulfate to beryllium silicate. First, after the beryllium-containing environmental slag is roasted, the beryllium sulfate in the waste residue is decomposed to form beryllium silicate to wrap the remaining beryllium sulfate, reduce the leaching toxic beryllium content, and play a role in fixing beryllium; secondly, the addition of auxiliary material C for roasting can reduce the S content in the slag, allowing S to enter the flue gas in the form of gaseous SO2, which plays a role in reducing the desulfurization roasting temperature and improving the desulfurization efficiency. The reduction of sulfur in the roasted sample can increase the proportion of cement clinker.
[0013] In the present invention, if the weight ratio of auxiliary materials added to the beryllium-containing environmentally friendly slag is less than 2%, the reaction will be incomplete and some of the beryllium-containing environmentally friendly slag will remain unreacted; if the weight ratio of auxiliary materials added to the beryllium-containing environmentally friendly slag is higher than 10%, some of the auxiliary materials will remain unreacted and too much auxiliary materials will remain; therefore, the weight ratio of auxiliary materials added to the beryllium-containing environmentally friendly slag is 2% to 10%.
[0014] As an optional implementation, in the resource recovery disposal method provided by the present invention, the amount of the auxiliary material added is 2 to 8% of the mass of the beryllium-containing environmentally friendly slag.
[0015] As an optional implementation, in the resource recovery disposal method provided by the present invention, the amount of the auxiliary material added is 2-6% of the mass of the beryllium-containing environmentally friendly slag.
[0016] As an optional implementation, in the resource recovery disposal method provided by the present invention, the beryllium-containing environmentally friendly slag is a precipitated slag formed after the beryllium-containing wastewater generated in the beryllium oxide production process is treated with lime milk.
[0017] As an optional embodiment, in the resource recovery disposal method provided by the present invention, the beryllium-containing environmentally friendly slag has a beryllium content of less than 0.4%, a sulfur content of less than 15%, a silicon dioxide content of greater than 15%, and a calcium oxide content of greater than 25%, measured by weight percentage, and is a hazardous waste.
[0018] In the present invention, beryllium in the beryllium-containing environmentally friendly slag is determined by ICP alkali fusion method, S is determined by high-frequency infrared absorption method, SiO2 is determined by perchloric acid dehydration weight method, and CaO is determined by atomic absorption spectrometry.
[0019] As an optional implementation, in the resource recovery disposal method provided by the present invention, the beryllium-containing environmentally friendly slag and auxiliary materials are roasted in a muffle furnace, and the power of the muffle furnace is 10kW to 20kW.
[0020] The muffle furnace used in the present invention is a box-type muffle furnace, which is a product currently sold on the market, such as a product sold under the trade name of exhaust-type high-temperature muffle furnace. The power of the box-type muffle furnace used in the present invention should be selected according to the heating rate.
[0021] As an optional implementation, in the resource recovery method provided by the present invention, the roasting time is 30 to 60 minutes.
[0022] In the present invention, the calcination time is set to 30 to 60 minutes. If the calcination time is less than 30 minutes, the reaction will be incomplete; if the calcination time is longer than 60 minutes, the energy consumption will increase.
[0023] As an optional implementation, in the resource recovery method provided by the present invention, the roasting time is 45 to 60 minutes.
[0024] As an optional implementation, in the resource recovery disposal method provided by the present invention, the content of toxic beryllium leached from the roasted sample is less than 0.00249 mg / L.
[0025] In the roasted sample obtained after roasting in the present invention, the content of leached toxic beryllium is less than 0.02 mg / l, which meets the treatment standard. The basic phase composition of beryllium is beryl, beryllium sulfate and beryllium silicate, and the beryllium in the product mainly exists in the form of beryllium silicate.
[0026] A second aspect of the present invention provides an application of the above-mentioned resource disposal method of beryllium-containing environmentally friendly slag in the preparation of cement clinker admixtures, specifically, the roasted sample obtained after the treatment is used to prepare cement clinker admixtures.
[0027] As an optional implementation, in the application provided by the present invention, the mixing ratio of the roasted sample in the M32.5 cement is 19.5%.
[0028] As an optional implementation, in the resource recovery disposal method provided by the present invention, the mixing ratio of the roasted sample in the M42.5 cement is 14.5%.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The present invention adopts a method for roasting beryllium-containing environmentally friendly slag and a reducing coal auxiliary material, and the content of leached toxic beryllium in the obtained roasted sample is less than 0.02 mg / L. The obtained roasted sample can also be used as an admixture for cement clinker, so that the beryllium-containing environmentally friendly slag is disposed of as a resource. The roasting disposal process adopted in the present invention is simple, with low equipment investment, low operating cost, good curing effect of the roasted product, no three wastes generated, and low environmental pollution, which meets the requirements of safe, efficient and green disposal of beryllium-containing environmentally friendly slag. DETAILED DESCRIPTION
[0031] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in combination with the contents of the specification and preferred embodiments, but the protection scope of the present invention is not limited to the following specific embodiments.
[0032] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0033] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0034] 1. Resource disposal method of environmentally friendly slag containing beryllium
[0035] Example 1
[0036] The resource disposal method of beryllium-containing environmental slag is as follows:
[0037] (1) Add auxiliary materials
[0038] The environmentally friendly silicon slag in this embodiment is the environmentally friendly beryllium-containing slag obtained by Minmetals Beryllium Industry Co., Ltd., and its components are analyzed. Its chemical composition is 0.28% Be, 12.65% S, 21.50% SiO2 and 32.00% CaO by weight. The auxiliary material is reducing coal, of which fixed carbon is 56.80% and calorific value is 4850kcal / kg.
[0039] According to the weight ratio of 4% of the auxiliary material added to the beryllium-containing environmentally friendly slag, the beryllium-containing environmentally friendly slag and the auxiliary material coal are evenly mixed to obtain the beryllium-containing environmentally friendly slag containing the auxiliary material.
[0040] (2) Calcination
[0041] The beryllium-containing environmentally friendly slag obtained in step (1) and the auxiliary material mixture were calcined at 950° C. for 30 min using an exhaust-type high-temperature box muffle furnace to obtain a calcined sample. The leaching toxicity of beryllium in the product obtained by this method was 0.0001 mg / L, which was lower than the standard of 0.02 mg / L.
[0042] Example 2
[0043] The resource disposal method of beryllium-containing environmental slag is as follows:
[0044] (1) Add auxiliary materials
[0045] The beryllium-containing environmental slag in this embodiment is obtained by Minmetals Beryllium Industry Co., Ltd., and its chemical composition is 0.12% Be, 12.75% S, 40.33% SiO2 and 14.55% CaO by weight. The auxiliary material is reducing coal, of which fixed carbon is 56.58% and calorific value is 4599kcal / kg.
[0046] According to the weight ratio of the auxiliary material added to the beryllium-containing environmentally friendly slag being 10%, the beryllium-containing environmentally friendly slag and the auxiliary material coal are evenly mixed to obtain the beryllium-containing environmentally friendly slag containing the auxiliary material.
[0047] (2) Calcination
[0048] The beryllium-containing environmentally friendly slag obtained in step (1) and the auxiliary material mixture were calcined at 950° C. for 45 min using an exhaust-type high-temperature box muffle furnace to obtain a calcined sample. The leaching toxicity of beryllium in the product obtained by this method was 0.00031 mg / L, which was lower than the standard of 0.02 mg / L.
[0049] Example 3
[0050] The resource disposal method of beryllium-containing environmental slag is as follows:
[0051] (1) Add auxiliary materials
[0052] The beryllium-containing environmentally friendly slag in this embodiment is obtained by Minmetals Beryllium Industry Co., Ltd., and its chemical composition is 0.30% Be, 12.67% S, 19.55% SiO2 and 32.35% CaO by weight. The fixed carbon in the auxiliary material is 55.33% and the calorific value is 4739kcal / kg.
[0053] According to the weight ratio of 7% of the auxiliary materials added to the beryllium-containing environmentally friendly slag, the beryllium-containing environmentally friendly slag and the auxiliary material coal are evenly mixed to obtain the beryllium-containing environmentally friendly slag containing the auxiliary materials.
[0054] (2) Calcination
[0055] The beryllium-containing environmentally friendly slag obtained in step (1) and the auxiliary material mixture were calcined at 1050° C. for 60 min using an exhaust-type high-temperature box muffle furnace to obtain a calcined sample. The leaching toxicity of beryllium in the product obtained by this method was 0.0001 mg / L, which was lower than the standard of 0.02 mg / L.
[0056] Example 4
[0057] The resource disposal method of beryllium-containing environmental slag is as follows:
[0058] (1) Add auxiliary materials
[0059] The beryllium-containing environmentally friendly slag in this embodiment is obtained by Minmetals Beryllium Industry Co., Ltd., and its components are analyzed. Its chemical composition is 0.23% Be, 13.69% S, 23.95% SiO2 and 30.05% CaO by weight. The fixed carbon in the auxiliary material is 56.65% and the calorific value is 4689kcal / kg.
[0060] According to the weight ratio of 4% of the auxiliary material added to the beryllium-containing environmentally friendly slag, the beryllium-containing environmentally friendly slag and the auxiliary material coal are evenly mixed to obtain the beryllium-containing environmentally friendly slag containing the auxiliary material.
[0061] (2) Calcination
[0062] The beryllium-containing environmentally friendly slag obtained in step (1) and the auxiliary material mixture were calcined at 900° C. for 30 min using an exhaust-type high-temperature box muffle furnace to obtain a calcined sample. The leaching toxicity of beryllium in the product obtained by this method was 0.00249 mg / L, which was lower than the standard of 0.02 mg / L.
[0063] Example 5
[0064] The resource disposal method of beryllium-containing environmental slag is as follows:
[0065] (1) Add auxiliary materials
[0066] The beryllium-containing environmentally friendly slag in this embodiment is obtained by Minmetals Beryllium Industry Co., Ltd., and its components are analyzed. Its chemical composition is 0.29% Be, 12.85% S, 19.32% SiO2 and 29.68% CaO by weight. The fixed carbon in the auxiliary material is 56.40% and the calorific value is 4822kcal / kg.
[0067] According to the weight ratio of the auxiliary material added to the beryllium-containing environmentally friendly slag being 2%, the beryllium-containing environmentally friendly slag and the auxiliary material coal are evenly mixed to obtain the beryllium-containing environmentally friendly slag containing the auxiliary material.
[0068] (2) Calcination
[0069] The beryllium-containing environmentally friendly slag obtained in step (1) and the auxiliary material mixture were calcined at 950° C. for 30 min using an exhaust-type high-temperature box muffle furnace to obtain a calcined sample. The leaching toxicity of beryllium in the product obtained by this method was 0.0023 mg / L, which was lower than the standard of 0.02 mg / L.
[0070] Comparative Example 1
[0071] The resource disposal method of beryllium-containing environmental slag is as follows:
[0072] A. Ingredients
[0073] The beryllium-containing environmentally friendly slag of Example 1 is used. The beryllium-containing environmentally friendly slag is directly loaded into a corundum crucible without adding auxiliary materials.
[0074] B. Roasting
[0075] The beryllium-containing environmentally friendly slag obtained in step A was calcined at 950° C. for 30 minutes using an exhaust-type high-temperature box muffle furnace. The obtained product was analyzed. The leaching toxic beryllium of the product obtained by this method was 0.032 mg / L, which was higher than the standard of 0.02 mg / L.
[0076] Comparative Example 2
[0077] The resource disposal method of beryllium-containing environmental slag is as follows:
[0078] A. Ingredients
[0079] The beryllium-containing environmentally friendly slag of Example 2 is used. The beryllium-containing environmentally friendly slag is directly loaded into a corundum crucible without adding auxiliary materials.
[0080] B. Roasting
[0081] The beryllium-containing environmentally friendly slag obtained in step A was calcined at 950° C. for 45 minutes using an exhaust-type high-temperature box muffle furnace. The obtained product was analyzed. The leaching toxic beryllium of the product obtained by this method was 0.028 mg / L, which was higher than the standard of 0.02 mg / L.
[0082] Comparative Example 3
[0083] The resource disposal method of beryllium-containing environmental slag is as follows:
[0084] A. Ingredients
[0085] The beryllium-containing environmentally friendly slag of Example 3 is used. The beryllium-containing environmentally friendly slag is directly loaded into the corundum crucible without adding auxiliary materials.
[0086] B. Roasting
[0087] The beryllium-containing environmentally friendly slag obtained in step A was calcined at 1050° C. for 60 min using an exhaust-type high-temperature box muffle furnace. The obtained product was analyzed and the leaching toxic beryllium of the product obtained by this method was 0.052 mg / L, which was higher than the standard of 0.02 mg / L.
[0088] 2. Performance Testing
[0089] The calcined product obtained in Example 5 was subjected to acid and alkali liquid chemical analysis of different strengths to obtain phase composition analysis, and the results are shown in Appendix 1.
[0090] Table 1: Phase analysis of beryllium in the calcined product of Example 5 / %
[0091] Phase Beryllium in Beryl Beryllium in Beryllium Sulfate Beryllium in Beryllium Silicate Total Beryllium content 0.043 0.0001 0.33 0.37 Distribution rate 11.62 0.03 88.35 100
[0092] It can be seen from Table 1 that after the beryllium-containing environmentally friendly slag is roasted with auxiliary coal, the basic phase composition of beryllium in the product is beryl, beryllium sulfate, and beryllium silicate, and the beryllium in the product mainly exists in the form of beryllium silicate.
[0093] The calcined product obtained in Example 5 is used as a cement clinker admixture. The auxiliary material ratio and performance analysis are shown in Table 2.
[0094] Table 2: Performance test and analysis results of the calcined product used as cement clinker admixture in Example 5
[0095]
[0096]
[0097] It can be seen from Table 2 that the proportion of the calcined sample prepared in Example 1 in the M32.5 type of cement can reach 19.5%, and the proportion in the M42.5 type of cement can reach 14.5%, and the setting time and compressive and flexural strengths of the cement all meet the requirements.
[0098] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.
Claims
1. A method for resource disposal of beryllium-containing environmentally friendly slag, characterized in that: The steps include: S1. Evenly mixing beryllium-containing environmentally friendly slag with auxiliary materials to obtain beryllium-containing environmentally friendly slag with auxiliary materials, wherein the auxiliary materials are added in an amount of 2 to 10% by mass of the beryllium-containing environmentally friendly slag; The beryllium-containing environmental slag is a precipitated slag formed after the beryllium-containing wastewater generated in the beryllium oxide production process is treated with lime milk; the auxiliary material is a reducing coal with a fixed carbon content greater than 55% and a calorific value greater than 4000kcal / kg; S2. The beryllium-containing environmentally friendly slag mixed in S1 is calcined at 850° C. to 1000° C. to obtain a calcined sample; the leached toxic beryllium content in the calcined sample is less than 0.00249 mg / L, and the beryllium phase in the calcined sample is mainly beryllium silicate.
2. The method for recycling beryllium-containing environmental slag according to claim 1, characterized in that: The beryllium-containing environmentally friendly slag has, by weight percentage, a beryllium content of less than 0.4%, a sulfur content of less than 15%, a silicon dioxide content of more than 15%, and a calcium oxide content of more than 25%.
3. The method for recycling beryllium-containing environmental slag according to claim 1, characterized in that: The moisture content of the beryllium-containing environmentally friendly slag is 35% to 45%.
4. The method for recycling beryllium-containing environmental slag according to claim 1, characterized in that: The beryllium-containing environmentally friendly slag and auxiliary materials are roasted in a muffle furnace, and the power of the muffle furnace is 10kW to 20kW.
5. The method for recycling beryllium-containing environmental slag according to claim 1, characterized in that: The roasting time is 30 to 60 minutes.
6. Application of the beryllium-containing environmentally friendly slag resource disposal method according to any one of claims 1 to 5 in the preparation of cement clinker admixtures, characterized in that: The calcined samples obtained after treatment were used to prepare cement clinker admixtures.
7. The use according to claim 6, characterized in that The calcined sample is mixed in the M32.5 cement at a ratio of 19.5% and in the M42.5 cement at a ratio of 14.5%.
Citation Information
Patent Citations
A method for harmlessly disposing of beryllium slag
CN109706327B
Beryllium slag detoxification and co-processing resource utilization system and technology in cement kilns
CN109761514B
Harmless treatment method of beryllium-containing waste residues
CN110252761A