A production process and smelting equipment for lithium-boron alloy strip

By mixing boron powder with lithium carbide powder and stirring in lithium-magnesium melt, the problem of incomplete melting of boron powder in lithium boron alloy smelting is solved, and the uniformity of lithium content and the quality of lithium boron alloy tape is improved. Simplify production processes and reduce costs.

CN116144956BActive Publication Date: 2024-11-01SHANDONG ZHONGSHAN PHOTOELECTRIC MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310027855.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-09
Publication Date
2024-11-01
Estimated Expiration
2043-01-09

AI Technical Summary

Technical Problem

Incomplete melting of boron powder during the lithium boron alloy smelting process leads to violent exothermic heat, uncontrollable reaction rate and reaction temperature, resulting in uneven lithium content, affecting the quality and yield of the lithium boron alloy belt.

Method used

By mixing boron powder with lithium carbide powder and ball milling into a mixed powder of 50 to 100 μm, preheating in the preheating silo, adding lithium-magnesium melt to stir, controlling the reaction temperature and rate, forming a uniform lithium-boron alloy blocks, followed by curing and rolling into strips.

Benefits of technology

The uniformity of lithium content is improved, the complexity of subsequent processing is reduced, the uniformity and yield of lithium boron alloy tape is improved, the production cost is reduced, and the operation process is simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116144956B_ABST
    Figure CN116144956B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium-boron alloy strip production, and in particular to a production process and smelting equipment for a lithium-boron alloy strip. In the production process of the lithium-boron alloy strip, the raw materials include, by mass percentage, 20% to 50% of boron powder, 0.2% to 1% of lithium carbide powder, 50% to 80% of lithium, and 2% to 6% of magnesium. The specific steps include: (1) mixing the boron powder and the lithium carbide powder, ball milling and preheating; (2) melting lithium and magnesium at 400° C., heating to 440 to 460° C., adding the preheated mixed powder to the lithium-magnesium melt, and continuing to stir until the melt becomes viscous; (4) pouring all the melt into a preheated solidification crucible, heating to 500 to 560° C., keeping the temperature until the melt is completely solidified to obtain a lithium-boron alloy block, stopping heating, and cooling to 250° C.; (5) taking out the lithium-boron alloy block, naturally cooling it to room temperature, and sealing and packaging it; (6) putting the lithium-boron alloy block into a roller mill for multi-roll continuous rolling to obtain a lithium-boron alloy strip. The lithium-boron alloy strip prepared by the invention has uniform lithium content, good surface quality, no inclusions and discoloration, and high yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium-boron alloy strip production, and in particular to a production process and smelting equipment for a lithium-boron alloy strip. Background Art

[0002] Lithium-boron alloy is an ideal negative electrode material for lithium-based thermal batteries. It has outstanding advantages such as high specific energy, high specific power, low polarization, electrochemical potential similar to that of pure lithium, and the ability to maintain a stable structure above 600°C. When used as a negative electrode material for thermal batteries, it can significantly improve the specific capacity and specific power of thermal batteries. The volume and mass of thermal batteries of the same capacity are reduced by 10% to 30%, which effectively improves the performance of thermal batteries and provides an effective material guarantee for the replacement of thermal batteries.

[0003] During the smelting process of lithium-boron alloy, it undergoes complex changes in physical and chemical states. The raw material ratio, heat control and stirring conditions will affect the final phase structure, which is prone to various defects such as inclusions, holes, segregation, etc. The subsequent extrusion or rolling production methods will aggravate the internal component segregation and make it difficult to control the uniformity of the lithium content in each part, thus leading to differences in thermal stability and discharge capacity between the same batches.

[0004] Chinese patent CN102851561A discloses a lithium-boron alloy production process and equipment, wherein lithium and boron are mixed and heated to 400°C in a high-purity argon atmosphere for stirring and reaction for 2 hours, then heated to 450°C to form an alloy melt and cast into a mold, and then heated to 650°C for reaction for 1 hour until hardened, and the alloy ingot is demolded and packaged after cooling to room temperature. However, when boron powder is directly added to lithium for melting, the boron powder is easily incompletely melted, causing violent heat release, uncontrollable reaction rate and reaction temperature, resulting in uneven lithium content of lithium-boron alloy ingots, and large deviations in lithium content of lithium-boron alloy strips produced by rolling, which seriously affects the quality and yield of lithium-boron alloy strips. Summary of the invention

[0005] In view of the technical problems in the lithium-boron alloy production process, such as incomplete melting of boron powder, violent heat release, and uncontrollable reaction rate and reaction temperature, the present invention provides a lithium-boron alloy strip production process and smelting equipment.

[0006] In a first aspect, the present invention provides a production process for a lithium-boron alloy strip, wherein the raw materials include, by mass percentage, 20% to 50% boron powder, 0.2% to 1% lithium carbide powder, 50% to 80% lithium, and 2% to 6% magnesium; the process specifically comprises the following steps:

[0007] (1) Boron powder and lithium carbide powder are mixed, ball-milled into a mixed powder with a particle size of 50 to 100 μm, and added into a preheating bin and preheated to 200° C.;

[0008] (2) adding lithium to a melting crucible, heating to 400-440° C., adding magnesium after the lithium is completely melted, and stirring for 30-60 minutes to form a lithium-magnesium melt with a bright surface and no impurities;

[0009] (3) Heat the lithium-magnesium melt to 440-460°C, add the preheated mixed powder into the lithium-magnesium melt, and continue stirring until the melt becomes viscous:

[0010] (4) pouring all the melt into a solidification crucible preheated to 440-460° C., heating to 500-560° C. at a rate of 1° C. / min, smelting until the melt is completely solidified to obtain a lithium-boron alloy block, stopping heating, and cooling to 250° C. with the furnace;

[0011] (5) taking the lithium-boron alloy block out of the solidification crucible, cooling it naturally to room temperature, and sealing it;

[0012] (6) placing the lithium-boron alloy block into a rolling mill for multi-roll continuous rolling to obtain a lithium-boron alloy strip, which is then rolled up after trimming.

[0013] During the smelting process, the boron powder and lithium carbide powder are made into a mixed powder and preheated in advance, which helps to completely melt the boron powder and avoid the violent exothermic reaction between the boron powder and the lithium-magnesium melt, so that the reaction rate and reaction temperature can be controlled, and a melt with uniform lithium content is obtained, which is solidified to form a lithium-boron alloy block with uniform Li7B6+Li phase.

[0014] Furthermore, in step (3), the mass of the mixed powder added is 30% to 50% of the mass of the lithium-magnesium melt.

[0015] Furthermore, in step (3), the stirring speed is 200 to 600 rpm, and the stirring time is 60 to 240 min.

[0016] Furthermore, in step (6), the rolling amount of each pass is controlled between 10% and 20%.

[0017] Furthermore, steps (1) to (5) are carried out in a glove box with a water and oxygen content of less than 0.1 ppm and a high-purity argon atmosphere, and the rolling process of step (6) is carried out in a drying room with a dew point temperature below -45°C.

[0018] In a second aspect, the present invention provides a lithium-boron alloy smelting equipment for the above-mentioned production process, including a glove box, wherein two independent temperature-controlled furnace bodies are arranged in the glove box, and a smelting crucible and a solidifying crucible are arranged on the two independent temperature-controlled furnace bodies respectively, and stirring devices are arranged in the smelting crucible and the solidifying crucible respectively, and a preheating bin is also arranged on the top of the smelting crucible.

[0019] Furthermore, the preheating silo is made of stainless steel, and the heating method is electric heating, and the heating temperature can be 100-300°C.

[0020] Furthermore, a temperature control system is provided in the independent temperature-controlled furnace, and the temperature measuring element of the temperature control system is a thermocouple.

[0021] Furthermore, the heating method of the independent temperature-controlled furnace body is electromagnetic induction heating or resistance heating.

[0022] Furthermore, the melting crucible and the solidifying crucible are made of ferritic stainless steel.

[0023] The beneficial effects of the present invention are:

[0024] The production process of the lithium-boron alloy strip provided by the present invention adds lithium carbide powder so that the boron powder and the lithium-magnesium melt do not generate intense heat, the reaction rate and reaction temperature are controllable, and a lithium-boron alloy block with uniform lithium content is obtained. After smelting, the next rolling process can be directly carried out without subsequent complex processing. The uniformity of the obtained lithium-boron alloy strip is improved, the deviation of lithium content in different parts of the same batch is controlled within 1%, the surface quality is good, there is no inclusion and discoloration, the yield is high, the operation is simple, and continuous production can be achieved without the need for additional large-scale extrusion or pier pressing equipment, which reduces production costs and improves labor efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0026] Figure 1 It is a structural schematic diagram of the lithium-boron alloy smelting equipment in the embodiment of the present application.

[0027] Among them, 1. glove box; 2. furnace body; 3. thermocouple; 4. melting crucible; 5. solidification crucible; 6. stirring device; 7. preheating silo. DETAILED DESCRIPTION

[0028] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0029] Example 1

[0030] A lithium-boron alloy smelting equipment includes a glove box 1, in which two independently temperature-controlled furnace bodies 2 are arranged. The furnace body 2 is heated by a variable frequency resistance heating wire, and ceramic is used as a heat-insulating material inside the furnace body 2. The temperature control system inside the furnace body 2 detects the center temperature of the furnace body through a thermocouple 3, and automatically adjusts the heating power according to preset parameters to achieve temperature control. A smelting crucible 4 and a solidifying crucible 5 are respectively arranged on the two independently temperature-controlled furnace bodies 2, and the smelting crucible 4 and the solidifying crucible 5 are both made of ferritic stainless steel. A stirring device 6 is respectively arranged in the smelting crucible 4 and the solidifying crucible 5, and a preheating bin 7 is also arranged on the upper part of the smelting crucible 4.

[0031] The lithium-boron alloy strip is produced by using the above lithium-boron alloy smelting equipment and rolling mill. The production process includes the following steps:

[0032] (1) 43 g of pre-dried and weighed boron powder and 1 g of lithium carbide powder were mixed evenly, and the mixed powder with a particle size of 50 to 100 μm was added to a preheating bin and preheated to 200° C.;

[0033] (2) In a glove box with a water and oxygen content of less than 0.1 ppm and a high-purity argon atmosphere, 58 g of lithium was weighed and placed in a melting crucible, and the temperature was kept at 440° C. After the lithium was completely melted, 4 g of magnesium was added, and a stirring device was installed. The mixture was stirred for 30 minutes to obtain a lithium-magnesium melt with a bright surface and no impurities;

[0034] (3) Add the preheated mixed powder into the lithium-magnesium melt and continue stirring at a stirring speed of 200 rpm. When the melt becomes sticky, remove the stirring paddle and stir for 60 min.

[0035] (4) preheating the solidification crucible to 440°C in advance, pouring all the melt into the solidification crucible, and then heating the solidification crucible to 560°C at a rate of 1°C / min, keeping the temperature until the melt is completely solidified to obtain a lithium-boron alloy block, stopping heating, and cooling with the furnace to 250°C;

[0036] (5) knocking out the lithium-boron alloy block, naturally cooling it to room temperature in a glove box, vacuum-sealing it, and transferring it to a drying room with a dew point of -45°C;

[0037] (6) According to product requirements, the lithium-boron alloy block is placed in a rolling mill for multi-roll continuous rolling, and the rolling amount of each pass is controlled at 10%. After 15 passes of rolling, a lithium-boron alloy strip with a thickness of 0.6 mm ± 0.03 mm is obtained, which is trimmed and rolled.

[0038] The lithium-boron alloy strip was cut into lithium-boron alloy sheet products of required specifications, and samples were taken to test the chemical composition, size, phase composition, density, appearance quality, thermal stability, and discharge performance of the products, and all passed the test; among them, the lithium content was determined to be in the range of 54.3% to 55.1%.

[0039] Example 2

[0040] The lithium-boron alloy strip is produced by using the lithium-boron alloy smelting equipment and rolling mill in Example 1. The production process includes the following steps:

[0041] 1) 32g of pre-dried and weighed boron powder and 0.5g of lithium carbide powder were mixed evenly, and the mixed powder with a ball-milled particle size of 50-100μm was added to the preheating bin and preheated to 200°C;

[0042] (2) In a glove box with a water and oxygen content of less than 0.1 ppm and a high-purity argon atmosphere, 75 g of lithium was weighed and placed in a melting crucible, and the temperature was kept at 420° C. After the lithium was completely melted, 6 g of magnesium was added, and a stirring device was installed. The mixture was stirred for 60 minutes to obtain a lithium-magnesium melt with a bright surface and no impurities;

[0043] (3) Add the preheated mixed powder into the lithium-magnesium melt and continue stirring at a speed of 400 rpm. When the melt becomes sticky, remove the stirring paddle. The stirring time is 80 min.

[0044] (4) preheating the solidification crucible to 420°C in advance, pouring all the melt into the solidification crucible, and then heating the solidification crucible to 540°C at a rate of 1°C / min, keeping the temperature until the melt is completely solidified to obtain a lithium-boron alloy block, stopping heating, and cooling with the furnace to 250°C;

[0045] (5) knocking out the lithium-boron alloy block, naturally cooling it to room temperature in a glove box, vacuum-sealing it, and transferring it to a drying room with a dew point of -45°C;

[0046] (6) According to product requirements, the lithium-boron alloy block is placed in a rolling mill for multi-roll continuous rolling, and the rolling amount of each pass is controlled at 15%. After 12 passes of rolling, a lithium-boron alloy strip with a thickness of 0.6 mm ± 0.03 mm is obtained, which is trimmed and rolled.

[0047] The lithium-boron alloy strips were punched out into lithium-boron alloy disc products of required specifications. Samples were taken to test the chemical composition, size, phase composition, density, appearance quality, thermal stability and discharge performance of the products, and all passed the test. Among them, the lithium content measurement results were all within the range of 65.7% to 66.3%.

[0048] Example 3

[0049] The lithium-boron alloy strip is produced by using the lithium-boron alloy smelting equipment and rolling mill in Example 1. The production process includes the following steps:

[0050] 1) 38g of pre-dried and weighed boron powder and 0.7g of lithium carbide powder were mixed evenly, and the mixed powder with a ball-milled particle size of 50-100μm was added to the preheating bin and preheated to 200°C;

[0051] (2) In a glove box with a water and oxygen content of less than 0.1 ppm and a high-purity argon atmosphere, 72 g of lithium was weighed and placed in a melting crucible, which was kept at 400° C. After the lithium was completely melted, 4 g of magnesium was added, and a stirring device was installed. The mixture was stirred for 60 min to obtain a lithium-magnesium melt with a bright surface and no impurities;

[0052] (3) Add the preheated mixed powder into the lithium-magnesium melt and continue stirring at a stirring speed of 400 rpm. When the melt becomes sticky, remove the stirring paddle and stir for 100 min.

[0053] (4) preheating the solidification crucible to 400°C in advance, pouring all the melt into the solidification crucible, and then heating the solidification crucible to 520°C at a rate of 1°C / min, keeping the temperature until the melt is completely solidified to obtain a lithium-boron alloy block, stopping heating, and cooling with the furnace to 250°C;

[0054] (5) knocking out the lithium-boron alloy block, naturally cooling it to room temperature in a glove box, vacuum-sealing it, and transferring it to a drying room with a dew point of -45°C;

[0055] (6) According to product requirements, the lithium-boron alloy block is placed in a rolling mill for multi-roll continuous rolling, and the rolling amount of each pass is controlled at 20%. After 10 passes of rolling, a lithium-boron alloy strip with a thickness of 0.6 mm ± 0.03 mm is obtained, which is trimmed and rolled.

[0056] The lithium-boron alloy strips were punched out into lithium-boron alloy disc products of required specifications. Samples were taken to test the chemical composition, size, phase composition, density, appearance quality, thermal stability and discharge performance of the products, and all passed the test. Among them, the lithium content determination results were all within the range of 71.6% to 72.3%.

[0057] Comparative Example

[0058] The lithium-boron alloy strip is produced by using the lithium-boron alloy smelting equipment and rolling mill in Example 1. The production process includes the following steps:

[0059] (1) 68 g of lithium and 32 g of boron powder were mixed and placed in a melting crucible, kept at 400° C., and stirred for 60 min, and then heated to 450° C. to obtain a melt;

[0060] (2) Preheat the solidification crucible to 450° C., pour all the melt into the solidification crucible, raise the temperature to 650° C., keep the temperature for 60 min until solidification, obtain a lithium-boron alloy block, stop heating, and cool down to 250° C. with the furnace;

[0061] (3) knocking out the lithium-boron alloy block, naturally cooling it to room temperature in a glove box, vacuum-sealing it, and transferring it to a drying room with a dew point of -45°C;

[0062] (6) According to product requirements, the lithium-boron alloy block is placed in a rolling mill for multi-roll continuous rolling, and the rolling amount of each pass is controlled at 20%. After 10 passes of rolling, a lithium-boron alloy strip with a thickness of 0.6 mm ± 0.03 mm is obtained.

[0063] The lithium-boron alloy strip had severe cracking at the edge, an uneven surface, discoloration and inclusions, and a wide edge to be cut. The lithium-boron alloy strip was cut into sheets, and samples were taken to test the chemical composition of the sheets. The lithium content ranged from 63.4% to 79.2%.

[0064] Although the present invention is described in detail by combining the drawings and preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person skilled in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person skilled in the art who is familiar with the present technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, and they shall be within the protection scope of the present invention.

Claims

1. A production process for a lithium-boron alloy strip, characterized in that: In terms of mass percentage, the raw materials include 28.194% to 40.566% boron powder, 0.441% to 0.943% lithium carbide powder, 54.717% to 66.079% lithium, and 3.774% to 5.286% magnesium; specifically, the following steps are included: (1) After mixing boron powder and lithium carbide powder, ball-mill them into a mixed powder with a particle size of 50-100 μm, add them into a preheating bin and preheat them to 200°C; (2) Add lithium to the melting crucible and heat to 400-440°C. After the lithium is completely melted, add magnesium and stir for 30-60 minutes to form a lithium-magnesium melt with a bright surface and no impurities. (3) Heat the lithium-magnesium melt to 440-460°C, add the preheated mixed powder into the lithium-magnesium melt, and continue stirring until the melt becomes viscous; (4) Pour all the melt into a solidification crucible preheated to 440-460°C, heat it to 500-560°C at a rate of 1°C / min, and smelt it until the melt is completely solidified to obtain a lithium-boron alloy block. Stop heating and cool it down to 250°C with the furnace. (5) Take the lithium-boron alloy block out of the solidification crucible, cool it naturally to room temperature, and seal it; (6) The lithium-boron alloy block is placed in a rolling mill for multi-roll continuous rolling to obtain a lithium-boron alloy strip, which is then wound up after trimming.

2. The production process according to claim 1, characterized in that: In step (3), the mass of the mixed powder added is 30% to 50% of the mass of the lithium-magnesium melt.

3. The production process according to claim 1, characterized in that: In step (3), the stirring speed is 200-600 rpm, and the stirring time is 60-240 min.

4. The production process according to claim 1, characterized in that: In step (6), the rolling amount of each pass is controlled between 10% and 20%.

5. The production process according to claim 1, characterized in that: Steps (1) to (5) are carried out in a glove box with a water and oxygen content of less than 0.1 ppm and a high-purity argon atmosphere, and the rolling process of step (6) is carried out in a drying room with a dew point temperature below -45°C.

6. A lithium-boron alloy smelting equipment for the production process as claimed in claim 1, characterized in that: It comprises a glove box, in which two independent temperature-controlled furnace bodies are arranged, on which a melting crucible and a solidifying crucible are arranged respectively, stirring devices are arranged in the melting crucible and the solidifying crucible respectively, and a preheating bin is also arranged on the top of the melting crucible.

7. The lithium-boron alloy smelting equipment according to claim 6, characterized in that: The preheating silo is made of stainless steel and is heated by electricity, with a heating temperature of 100~300℃.

8. The lithium-boron alloy smelting equipment according to claim 6, characterized in that: A temperature control system is arranged in the independent temperature control furnace, and the temperature measuring element of the temperature control system is a thermocouple.

9. The lithium-boron alloy smelting equipment according to claim 6, characterized in that: The heating method of the independent temperature control furnace body is electromagnetic induction heating or resistance heating.

10. The lithium-boron alloy smelting equipment according to claim 6, characterized in that: Melting crucible and solidification crucible are made of ferritic stainless steel.