Multilayer ceramic electronic components

By forming Ni, Cr, Cu, and Ti thin film electrodes on the base electrode layer of the laminated ceramic electronic component, and adjusting the metal particle size of the Cu plating layer, the problem of cracks and moisture resistance degradation caused by thermal stress is solved, and a more advanced design is achieved. High stability and moisture resistance.

CN116153665BActive Publication Date: 2024-10-29MURATA MFG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310270683.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-16
Publication Date
2024-10-29
Estimated Expiration
2041-04-16

AI Technical Summary

Technical Problem

Existing laminated ceramic electronic components have problems with cracks in the external electrodes due to thermal stress during reflow soldering, and their moisture resistance deteriorates, making it impossible to effectively prevent moisture from infiltrating.

Method used

A thin film electrode whose base electrode layer is composed of Ni, Cr, Cu, Ti and other metals is used, and a Cu plating layer is formed on it. By adjusting the metal particle size of the plating layer, the compressive stress is reduced, the tensile stress is suppressed, and the Adhesion and moisture resistance.

Benefits of technology

It effectively suppresses cracks caused by thermal stress and improves moisture resistance, ensuring the stability and reliability of laminated ceramic electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116153665B_ABST
    Figure CN116153665B_ABST
Patent Text Reader

Abstract

The present invention provides a laminated ceramic electronic component. In the laminated ceramic capacitor, the external electrode has a base electrode layer, a lower plating layer arranged on the base electrode layer and arranged on the first end face and the second end face, and an upper plating layer arranged on the lower plating layer. The base electrode layer is a thin film electrode containing at least one selected from Ni, Cr, Cu, and Ti. The lower plating layer is composed of a Cu plating layer, and the lower plating layer has a lower region located on the laminate side and an upper region located between the lower region and the upper plating layer, and the metal particle size of the Cu plating layer located in the lower region is smaller than the metal particle size of the Cu plating layer located in the upper region.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an invention patent application with an application date of April 16, 2021, an application number of 202110415758.1, and an invention name of “Stacked Ceramic Electronic Components”. Technical Field

[0002] The present invention relates to a laminated ceramic electronic component, and in particular to a laminated ceramic electronic component having external electrodes of a multilayer structure. Background Art

[0003] In recent years, electronic devices such as mobile phones and portable music players have been miniaturized and thinned. Along with this, multilayer ceramic electronic components mounted in the miniaturized and thinned electronic devices have also been miniaturized and thinned.

[0004] A multilayer ceramic capacitor as such a multilayer ceramic electronic component, for example, as disclosed in Japanese Patent Application Laid-Open No. 8-306580, comprises a ceramic sintered body in which dielectric ceramics such as barium titanate and internal electrodes are alternately stacked, and a pair of external electrodes formed to cover each end surface of the ceramic sintered body (see Japanese Patent Application Laid-Open No. 8-306580).

[0005] As one of the methods for achieving miniaturization and high capacitance, there is a technique for forming external electrodes using plated electrodes (Cu plating) as disclosed in Japanese Patent Application Laid-Open No. 2009-283597. In Japanese Patent Application Laid-Open No. 8-306580, the thickness of the external electrodes is reduced by directly forming plated electrodes (Cu plating) on ​​the electronic component body, and the ceramic body can be made as large as possible within the standard size to increase the effective area of ​​the internal electrodes in accordance with the thinning of the external electrodes.

[0006] However, when a plated electrode (Cu plating layer) is formed on a ceramic body as in Japanese Unexamined Patent Publication No. 2009-283597, it is known that there is a problem in that the adhesion with the ceramic laminate and the internal electrode is insufficient, moisture penetrates from the outside, and moisture resistance deteriorates.

[0007] Therefore, as a solution to this problem, a method of increasing the particle size of the metal of the plating electrode by performing heat treatment after forming the plating electrode (Cu plating layer) and increasing the contact area with the ceramic body to ensure adhesion can be considered.

[0008] However, when the particle size of the metal of the plating electrode (Cu plating) is increased by heat treatment, the compressive stress of the particles themselves becomes large, so the compressive stress of the plating electrode (Cu plating) itself becomes large. Here, the external electrode is formed on the first main surface and the second main surface, the first side surface and the second side surface, and the first end surface and the second end surface, so the front end of the plating electrode (Cu plating) formed on the first main surface and the second main surface, the first side surface and the second side surface is in a state of tensile stress. In this state, if thermal stress is applied (for example, ΔT230°C during solder reflow installation, and ΔT140°C or more and 180°C or less if it is a thermal shock of the product after installation), the tensile force will be concentrated at the front end of the plating electrode (Cu plating). Therefore, it can be considered that for the ceramic body, the force in the perpendicular direction to the direction of the tensile stress of the external electrode is applied to the front end of the plating electrode (Cu plating), so cracks will be generated in the ceramic body due to thermal stress. In addition, this problem occurs more significantly as the thickness of the ceramic body becomes thinner. Summary of the invention

[0009] Therefore, a main object of the present invention is to provide a multilayer ceramic electronic component capable of suppressing the occurrence of cracks in a multilayer body due to thermal stress during reflow soldering or the like.

[0010] The laminated ceramic electronic component of the present invention is a laminated ceramic electronic component comprising: a laminated body including a plurality of laminated ceramic layers, and having a first main surface and a second main surface opposite to each other in a height direction, a first side surface and a second side surface opposite to each other in a width direction perpendicular to the height direction, and a first end surface and a second end surface opposite to each other in a length direction perpendicular to the height direction and the width direction; a first internal electrode layer arranged on the ceramic layer and exposed at the first end surface; a second internal electrode layer arranged on the ceramic layer and exposed at the second end surface; a first external electrode connected to the first internal electrode layer and arranged on the first end surface; and a second external electrode layer. , connected to the second internal electrode layer and arranged on the second end face, wherein the first external electrode and the second external electrode have a base electrode layer, a lower plating layer arranged on the base electrode layer and arranged on the first end face and the second end face, and an upper plating layer arranged on the lower plating layer, the base electrode layer is a thin film electrode containing at least one selected from Ni, Cr, Cu, and Ti, the lower plating layer is composed of a Cu plating layer, the lower plating layer has a lower region located on the stack side and an upper region located between the lower region and the upper plating layer, and the metal particle size of the Cu plating layer located in the lower region is smaller than the metal particle size of the Cu plating layer located in the upper region.

[0011] According to the laminated ceramic electronic component of the present invention, the first external electrode and the second external electrode have a base electrode layer, a lower plating layer arranged on the base electrode layer and arranged on the first end surface and the second end surface, and an upper plating layer arranged on the lower plating layer, the base electrode layer is a thin film electrode containing at least one selected from Ni, Cr, Cu, and Ti, the lower plating layer is composed of a Cu plating layer, the lower plating layer has a lower region located on the laminated body side and an upper region located between the lower region and the upper plating layer, the metal particle size of the Cu plating layer located in the lower region is smaller than the metal particle size of the Cu plating layer located in the upper region, so that the adhesion with the laminated body can be ensured by the base electrode layer formed by the thin film layer, and the particle size of the metal particles constituting the lower region is small, so that the compressive stress of the entire lower plating layer can be reduced. As a result, even when thermal stress is applied, the tensile stress applied to the front end of the lower plating layer can be suppressed, and cracks generated in the laminated body due to the thermal stress can be suppressed.

[0012] Furthermore, according to the laminated ceramic electronic component of the present invention, in the upper region of the lower plating layer, the particle size of the metal particles constituting the upper region is larger than the particle size of the metal particles constituting the lower region, so that the thickness of the lower plating layer can be ensured, and the infiltration of moisture into the laminate can be suppressed. As a result, the deterioration of moisture resistance reliability can also be effectively exerted.

[0013] The above and other objects, features, aspects and advantages of the present invention will become apparent from the following detailed description of the present invention when read in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 FIG. 1 is a perspective view showing the appearance of a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to the first embodiment of the present invention.

[0015] Figure 2 It is a front view showing a multilayer ceramic capacitor as an example of the multilayer ceramic electronic component according to the first embodiment of the present invention.

[0016] Figure 3 It is a plan view showing a multilayer ceramic capacitor as an example of the multilayer ceramic electronic component according to the first embodiment of the present invention.

[0017] Figure 4 yes Figure 1 A cross-sectional view is concerned along line IV-IV.

[0018] Figure 5 yes Figure 1 The cross-sectional view is taken along line VV.

[0019] Figure 6 It is a schematic cross-sectional view for explaining the structure of the external electrode according to the present invention.

[0020] Figure 7 yes Figure 1 The cross-sectional view refers to the line VII-VII.

[0021] Figure 8 This is a perspective view showing the appearance of a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a first modification of the first embodiment of the present invention.

[0022] Fig. 9 It is a front view showing a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a first modification of the first embodiment of the present invention.

[0023] Fig.10 It is a plan view showing a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a first modification of the first embodiment of the present invention.

[0024] Fig.11 yes Figure 1 The cross-sectional view refers to the line XI-XI.

[0025] Fig.12 yes Figure 1 The cross-sectional view refers to the line XII-XII.

[0026] Fig.13 yes Figure 1 A cross-sectional view is concerned along line XIII-XIII.

[0027] Fig.14 1 is a central front cross-sectional view showing a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a second modification of the embodiment of the present invention.

[0028] Fig.15 1 is a central front cross-sectional view showing a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a third modified example of the embodiment of the present invention.

[0029] Fig.16 FIG. 1 is a perspective view showing the appearance of a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a second embodiment of the present invention.

[0030] Fig.17 yes Fig.16 The cross-sectional view refers to the line XVII-XVII.

[0031] Fig.18 yes Fig.16 The cross-sectional view refers to the line XVIII-XVIII.

[0032] Fig.19 yes Fig.16 The cross-sectional view refers to the line XIX-XIX.

[0033] Fig. 20 yes Fig.16 An exploded perspective view of the stack shown.

[0034] Fig.21A Show Fig.16 FIG. 1 is a first internal electrode pattern of a multilayer ceramic capacitor shown in FIG.

[0035] Fig.21B Show Fig.16 FIG. 2 is a second internal electrode pattern of a multilayer ceramic capacitor shown in FIG.

[0036] Fig. 22 It is a schematic cross-sectional view for explaining the structure of the external electrode according to the present invention.

[0037] Fig.23 It is a schematic cross-sectional view for explaining the structure of the external electrode according to the present invention.

[0038] Fig.24A It is an external perspective view of a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a modification of the second embodiment of the present invention.

[0039] Fig. 24B It is a bottom view of a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a modification of the second embodiment of the present invention.

[0040] Fig.25 yes Fig.16 The external perspective view of a laminated body of a laminated ceramic capacitor shown in FIG.

[0041] Fig.26 is Fig.25 The stacked body shown is a perspective view of the outer appearance of a base electrode layer.

[0042] Fig. 27 is Fig.26 The laminate shown is a perspective view of the appearance of a plated layer. DETAILED DESCRIPTION

[0043] Hereinafter, a multilayer ceramic electronic component will be described using this embodiment as an example of the present invention.

[0044] A. First embodiment

[0045] 1. Multilayer ceramic capacitors

[0046] A multilayer ceramic capacitor 10 is described as an example of a multilayer ceramic electronic component according to an embodiment of the present invention. Figure 1 FIG. 1 is a perspective view showing the appearance of a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to the first embodiment of the present invention. Figure 2 It is a front view showing a multilayer ceramic capacitor as an example of the multilayer ceramic electronic component according to the first embodiment of the present invention. Figure 3 It is a plan view showing a multilayer ceramic capacitor as an example of the multilayer ceramic electronic component according to the first embodiment of the present invention. Figure 4 yes Figure 1 A cross-sectional view is concerned along line IV-IV. Figure 5 yes Figure 1 The cross-sectional view is taken along line VV. Figure 6 It is a schematic cross-sectional view for explaining the structure of the external electrode according to the present invention. Figure 7 yes Figure 1 The cross-sectional view refers to the line VII-VII.

[0047] The multilayer ceramic capacitor 10 includes a multilayer body 12 and an external electrode 24. Hereinafter, each structure will be described in the order of the multilayer body 12 and the external electrode 24.

[0048] The laminate 12 has a plurality of stacked ceramic layers 14 and a plurality of internal electrode layers 16. Furthermore, the laminate 12 includes a first main surface 12a and a second main surface 12b opposite to each other in the height direction x, a first side surface 12c and a second side surface 12d opposite to each other in the width direction y orthogonal to the height direction x, and a first end surface 12e and a second end surface 12f opposite to each other in the length direction z orthogonal to the height direction x and the width direction y. In the laminate 12, the corners and the ridges are rounded. In addition, the so-called corners are the portions where three adjacent surfaces of the laminate 12 intersect, and the so-called ridges are the portions where two adjacent surfaces of the laminate 12 intersect. In addition, the first main surface 12a and the second main surface 12b, the first side surface 12c and the second side surface 12d, and the first end surface 12e and the second end surface 12f may be partially or entirely formed with projections and depressions.

[0049] like Figure 4 as well as Figure 5 As shown, the stack 12 has, in the height direction x connecting the first main surface 12a and the second main surface 12b to each other,: an effective layer portion 15a in which a plurality of internal electrode layers 16 are opposed to each other; a first outer layer portion 15b1 formed by a plurality of ceramic layers 14 located between the first main surface 12a and the internal electrode layer 16 located closest to the first main surface 12a; and a second outer layer portion 15b2 formed by a plurality of ceramic layers 14 located between the second main surface 12b and the internal electrode layer 16 located closest to the second main surface 12b.

[0050] The first outer layer portion 15 b 1 is located on the first principal surface 12 a side of the laminate 12 , and is an aggregate of a plurality of ceramic layers 14 located between the first principal surface 12 a and the internal electrode layer 16 closest to the first principal surface 12 a .

[0051] The second outer layer portion 15 b 2 is located on the second main surface 12 b side of the laminate 12 , and is an aggregate of a plurality of ceramic layers 14 located between the second main surface 12 b and the internal electrode layer 16 closest to the second main surface 12 b .

[0052] The area sandwiched by the first outer layer 15b1 and the second outer layer 15b2 is the effective layer 15a. The number of stacked ceramic layers 14 is not particularly limited, but preferably includes 15 or more and 70 or less of the first outer layer 15b1 and the second outer layer 15b2. In addition, the thickness of the ceramic layer 14 is preferably 0.4 μm or more and 10 μm or less.

[0053] The ceramic layer 14 may be made of a dielectric material, for example. For example, dielectric ceramics containing a main component such as BaTiO3, CaTiO3, SrTiO3, or CaZnO3 may be used as the dielectric material. In addition, materials containing a secondary component such as a Mn compound, a Fe compound, a Cr compound, a Co compound, or a Ni compound added to these main components may also be used.

[0054] The size of the laminate 12 is not particularly limited, but preferably the size in the length direction z is 0.2 mm or more and 10 mm or less, the size in the width direction y is 0.1 mm or more and 10 mm or less, and the size in the height direction x is 30 μm or more and 200 μm or less. In particular, in the present embodiment, the effect is more exerted on the laminate 12 with a small size in the height direction x of the laminate 12. This is because the smaller the size of the laminate 12 in the height direction x of the laminate 12 is, the lower the mechanical strength of the laminate 12 is.

[0055] like Figure 4 as well as Figure 5 As shown, the internal electrode layer 16 includes a first internal electrode layer 16 a and a second internal electrode layer 16 b. The first internal electrode layer 16 a and the second internal electrode layer 16 b are alternately stacked with the ceramic layer 14 interposed therebetween.

[0056] The first internal electrode layer 16a is arranged on the surface of the ceramic layer 14. The first internal electrode layer 16a has a first opposing electrode portion 18a opposed to the second internal electrode layer 16b, and a first lead electrode portion 20a located on one end side of the first internal electrode layer 16a and extending from the first opposing electrode portion 18a to the first end surface 12e of the laminate 12. The first lead electrode portion 20a has an end portion led out to the first end surface 12e and exposed.

[0057] The shape of the first counter electrode portion 18a of the first internal electrode layer 16a is not particularly limited, but is preferably rectangular in plan view. However, the corners may be rounded in plan view, or the corners may be formed to be inclined (conical) in plan view. In addition, the shape may be a cone in plan view that is inclined toward one direction.

[0058] The shape of the first lead electrode portion 20a of the first internal electrode layer 16a is not particularly limited, but is preferably rectangular in plan view. However, the corners may be rounded in plan view, or the corners may be formed to be inclined (conical) in plan view. In addition, the shape may be a cone in plan view that is inclined toward one direction.

[0059] The width of the first counter electrode portion 18a of the first internal electrode layer 16a and the width of the first lead electrode portion 20a of the first internal electrode layer 16a may be formed to be the same width, or one of the widths may be formed to be narrower.

[0060] The second internal electrode layer 16b is arranged on the surface of a ceramic layer 14 different from the ceramic layer 14 on which the first internal electrode layer 16a is arranged. The second internal electrode layer 16a includes a second opposing electrode portion 18b opposed to the first internal electrode layer 16a, and a second lead electrode portion 20b located on one end side of the second internal electrode layer 16b and extending from the second opposing electrode portion 18b to the second end face 12f of the laminate 12. The end of the second lead electrode portion 20b is led out to the second end face 12f and exposed.

[0061] The shape of the second counter electrode portion 18b of the second internal electrode layer 16b is not particularly limited, but is preferably rectangular in plan view. However, the corners may be rounded in plan view, or the corners may be formed to be inclined (conical) in plan view. In addition, the shape may be a cone in plan view that is inclined toward one direction.

[0062] The shape of the second lead electrode portion 20b of the second internal electrode layer 16b is not particularly limited, but is preferably rectangular in plan view. However, the corners may be rounded in plan view, or the corners may be formed to be inclined (conical) in plan view. In addition, the shape may be a cone in plan view that is inclined toward one direction.

[0063] The width of the second counter electrode portion 18b of the second internal electrode layer 16b and the width of the second lead electrode portion 20b of the second internal electrode layer 16b may be formed to be the same width, or one of the widths may be formed to be narrower.

[0064] Furthermore, if Figure 4As shown, the stack 12 includes an end portion (hereinafter referred to as "L gap") 22b of the stack 12, and the end portion 22b of the stack 12 is formed between the end portion of the first internal electrode layer 16a on the opposite side to the first lead electrode portion 20a and the second end face 12f, and between the end portion of the second internal electrode layer 16b on the opposite side to the second lead electrode portion 20b and the first end face 12e.

[0065] like Figure 5 As shown, the stack 12 includes a side portion (hereinafter referred to as a "W gap") 22a of the stack 12, and the side portion 22a of the stack 12 is formed between one end of the first opposing electrode portion 18a and the second opposing electrode portion 18b in the width direction y and the first side surface 12c, and between the other end of the first opposing electrode portion 18a and the second opposing electrode portion 18b in the width direction y and the second side surface 12d.

[0066] The first internal electrode layer 16a and the second internal electrode layer 16b can include, for example, metals such as Ni, Cu, Ag, Pd, Au, or alloys containing at least one of these metals such as Ag-Pd alloys, etc. The internal electrode layer 16 may further include dielectric particles having the same composition as the ceramic contained in the ceramic layer 14.

[0067] When piezoelectric ceramics are used for the laminated body 12, the laminated ceramic electronic component functions as the ceramic piezoelectric element 10a. Specific examples of piezoelectric ceramic materials include PZT (lead zirconate titanate) based ceramic materials.

[0068] When semiconductor ceramics are used for the laminated body 12, the laminated ceramic electronic component functions as the thermistor element 10b. Specific examples of semiconductor ceramic materials include spinel ceramic materials.

[0069] When magnetic ceramic is used for the laminate 12, the laminated ceramic electronic component functions as the inductor element 10c. When it functions as an inductor element, the internal electrode layer becomes a coil-shaped conductor. Specific examples of magnetic ceramic materials include 0 material and the like.

[0070] That is, the multilayer ceramic electronic component according to the present embodiment can function appropriately not only as a multilayer ceramic capacitor 10 but also as a ceramic piezoelectric element 10a, a thermistor element 10b, or an inductor element 10c by appropriately changing the material and structure of the multilayer body 12.

[0071] The thickness of the internal electrode layer 16 , that is, the first internal electrode layer 16 a and the second internal electrode layer 16 b is preferably 0.2 μm or more and 2.0 μm or less.

[0072] Furthermore, the total number of the first internal electrode layers 16 a and the second internal electrode layers 16 b is preferably 15 or more and 200 or less.

[0073] The internal electrode layer 16 may be provided in parallel with the surface mounted on the mounting substrate or may be provided perpendicularly to the surface mounted on the mounting substrate, but is more preferably provided in parallel with the surface mounted on the mounting substrate.

[0074] like Figures 1 to 4 As shown in FIG. 1 , external electrodes 24 are arranged on the first end surface 12 e side and the second end surface 12 f side of the stacked body 12 .

[0075] The external electrode 24 includes a base electrode layer 26 and a plating layer 28 formed to cover the base electrode layer 26 .

[0076] The external electrode 24 includes a first external electrode 24 a and a second external electrode 24 b .

[0077] The first external electrode 24a is disposed only on the surface of the first end face 12e, a portion of the first main face 12a, and a portion of the second main face 12b of the stacked body 12. In this case, the first external electrode 24a is electrically connected to the first lead electrode portion 20a of the first internal electrode layer 16a. In addition, the first external electrode 24a is not disposed on a portion of the first side face 12c and a portion of the second side face 12d.

[0078] The second external electrode 24b is disposed only on the surface of the second end face 12f, a portion of the first main face 12a, and a portion of the second main face 12b of the stacked body 12. In this case, the second external electrode 24b is electrically connected to the second lead electrode portion 20b of the second internal electrode layer 16b. In addition, the second external electrode 24b is not disposed on a portion of the first side face 12c and a portion of the second side face 12d.

[0079] In the laminate 12, the first opposing electrode portion 18a of the first internal electrode layer 16a and the second opposing electrode portion 18b of the second internal electrode layer 16b are opposed to each other via the ceramic layer 14, thereby forming an electrostatic capacitor. Therefore, an electrostatic capacitor can be obtained between the first external electrode 24a connected to the first internal electrode layer 16a and the second external electrode 24b connected to the second internal electrode layer 16b, and the characteristics of a capacitor are exhibited.

[0080] The base electrode layer 26 includes a first base electrode layer 26a1, a second base electrode layer 26a2, a third base electrode layer 26b1, and a fourth base electrode layer 26b2. In order to further improve performance, the first base electrode layer 26a1, the second base electrode layer 26a2, the third base electrode layer 26b1, and the fourth base electrode layer 26b2 are formed of a thin film layer including a plurality of thin film electrodes.

[0081] The first foundation electrode layer 26a1 is formed so as to cover a portion of the first principal surface 12a on the first end surface 12e side of the laminate 12. The second foundation electrode layer 26a2 is formed so as to cover a portion of the second principal surface 12b on the first end surface 12e side of the laminate 12.

[0082] The third foundation electrode layer 26b1 is formed to cover a portion of the first principal surface 12a on the second end surface 12f side of the stacked body 12. The fourth foundation electrode layer 26b2 is formed to cover a portion of the second principal surface 12b on the second end surface 12f side of the stacked body 12.

[0083] The base electrode layer 26 formed of a thin film layer is preferably formed by a thin film forming method such as sputtering or evaporation. In particular, the base electrode layer 26 formed of a thin film layer is preferably a sputtering electrode formed by sputtering. The electrode formed by sputtering is described below.

[0084] When the base electrode layer 26 is formed by a sputtering electrode, it is preferable to directly form the sputtering electrode on a part of the first main surface 12 a and a part of the second main surface 12 b of the laminate 12 .

[0085] The base electrode layer 26 formed by the sputtering electrode contains at least one selected from Ni, Cr, Cu, Ti, and the like.

[0086] The thickness of the sputtering electrode in the height direction x connecting the first main surface 12 a and the second main surface 12 b is preferably 50 nm to 400 nm, and more preferably 50 nm to 130 nm.

[0087] The plating layer 28 includes a first plating layer 28 a and a second plating layer 28 b .

[0088] The first plating layer 28a is arranged to cover the first foundation electrode layer 26a1 and the second foundation electrode layer 26a2.

[0089] The second plating layer 28b is arranged to cover the third foundation electrode layer 26b1 and the fourth foundation electrode layer 26b2.

[0090] The plating layer 28 may be formed of a plurality of layers.

[0091] Preferably, the plating layer 28 includes a lower plating layer 30 covering the base electrode layer 26 and an upper plating layer 32 configured to cover the lower plating layer 30 .

[0092] Among the plating layers 28 , the upper plating layer 32 includes at least one selected from, for example, Ni, Sn, Cu, Ag, Pd, an Ag—Pd alloy, Au, and the like.

[0093] The lower plating layer 30 includes a first lower plating layer 30a and a second lower plating layer 30b. The lower plating layer 30 is disposed on the base electrode layer 26 and disposed on the first end surface 12e and the second end surface 12f.

[0094] The first lower plating layer 30a is arranged on the first end surface 12e of the laminate 12 where no foundation electrode layer is arranged, and is arranged to cover the first foundation electrode layer 26a1 arranged on the first main surface 12a and the second foundation electrode layer 26a2 arranged on the second main surface 12b.

[0095] The second lower plating layer 30b is arranged on the second end surface 12f of the laminate 12 where no foundation electrode layer is arranged, and is arranged to cover the third foundation electrode layer 26b1 arranged on the first main surface 12a and the fourth foundation electrode layer 26b2 arranged on the second main surface 12b.

[0096] This allows the plating thickness of the plating layers after the second layer (upper plating layer 32 ) to be uniform, and the effect of suppressing the variation in the plating thickness of the second layer (upper plating layer 32 ) can be achieved.

[0097] In the present embodiment, the metal contained in the lower plating layer 30 is Cu. Therefore, the lower plating layer 30 is formed as a Cu plating layer. Since the lower plating layer 30 is formed as a Cu plating layer and is provided to cover the surface of the base electrode layer 26, there is an effect of suppressing the infiltration of the plating solution.

[0098] Furthermore, if Figure 6 As shown, the lower plating layer 30 includes a lower region 40 located on the laminated body 12 side and an upper region 42 located between the lower region 40 and the upper plating layer 32 .

[0099] The particle size of the metal particles constituting the Cu plating layer in the lower region 40 is smaller than that of the metal particles constituting the Cu plating layer in the upper region 42. The particle size of the metal particles constituting the Cu plating layer means the maximum particle size in the thickness direction of the Cu plating layer.

[0100] Thus, by reducing the particle size of the metal particles constituting the lower region 40 of the lower plating layer 30, the compressive stress of the entire lower plating layer 30 can be reduced. As a result, even when thermal stress is applied, the tensile stress applied to the front end of the lower plating layer 30 can be suppressed, and cracks in the laminate 12 caused by the thermal stress can be suppressed. In addition, by making the particle size of the metal particles constituting the upper region 42 of the lower plating layer 30 larger than the particle size of the metal particles constituting the lower region 40, the thickness of the lower plating layer 30 can be ensured, and the infiltration of moisture into the laminate 12 can be suppressed. As a result, it is possible to maintain good moisture resistance reliability while reducing the stress caused by the application of thermal stress.

[0101] In addition, in the upper region 42 of the lower plating layer 30, the particle size of the metal particles constituting the upper region 42 is large, so tensile stress caused by thermal stress may sometimes be generated. However, because the particle size of the metal particles constituting the lower region 40 is small, the lower region 40 becomes a barrier layer, which can suppress cracks caused by the stress generated in the upper region 42.

[0102] The particle sizes of the metal particles of the Cu plating layer located in the lower region 40 of the lower plating layer 30 and the particle sizes of the metal particles of the Cu plating layer located in the upper region 42 of the lower plating layer 30 can be measured by the following method.

[0103] That is, regarding the particle size of the metal particles constituting each Cu plating layer located in the lower region 40 and the upper region 42 of the lower plating layer 30, the LT cross section at the 1 / 2W position of the multilayer ceramic capacitor 10 is exposed, and the cross section of the lower plating layer 30 is observed with an electron microscope. The magnification is preferably 20,000 times or more. Ten lines are drawn at equal intervals in the thickness direction of the observation surface as the cross section of the lower plating layer 30, and the maximum particle size of the metal particles on the lines is measured, and the average value thereof is calculated as the particle size.

[0104] The thickness of the lower region 40 of the lower plating layer 30 is preferably smaller than the thickness of the upper region 42 of the lower plating layer 30. As a result, the compressive stress on the laminate 12 generated in the lower plating layer 30 due to the application of the thermal cycle is reduced, and the effect of suppressing the generation of cracks in the laminate 12 caused by the compressive stress can be obtained.

[0105] The thickness of the lower region 40 of the lower plating layer 30 is preferably 0.2 μm or more and 1.0 μm or less. If the thickness of the lower region 40 of the lower plating layer 30 is less than 0.2 μm, the lower region 40 formed by Cu plating will be discontinuously formed, and for example, the moisture resistance reliability of the multilayer ceramic capacitor 10 cannot be guaranteed. On the other hand, if the thickness of the lower region 40 of the lower plating layer 30 is greater than 1.0 μm, there is a possibility that formation defects at the ends of the external electrodes due to plating growth may occur.

[0106] The thickness of the upper region 42 of the lower plating layer 30 is preferably 4.0 μm or more and 8.0 μm or less. If the thickness of the upper region 42 of the lower plating layer 30 is less than 4.0 μm, the upper region 42 formed by Cu plating will be discontinuously formed, and for example, the moisture resistance reliability of the multilayer ceramic capacitor 10 cannot be guaranteed. On the other hand, if the thickness of the upper region 42 of the lower plating layer 30 is greater than 8.0 μm, the thickness of the body becomes thinner according to the plating thickness, and the desired capacitance and strength cannot be achieved.

[0107] Preferably, the particle size of the metal particles constituting the lower region 40 of the lower plating layer 30 is 0.20 μm or less, and the particle size of the metal particles constituting the upper region 42 of the lower plating layer 30 is 0.50 μm or more. Thus, due to the stress relief effect of the lower region 40 of the lower plating layer 30, the compressive stress on the stack 12 caused by the application of thermal stress is reduced, and the generation of cracks in the stack 12 caused by the compressive stress can be suppressed. Furthermore, the metal particles constituting the upper region 42 of the lower plating layer 30 can achieve the effect of suppressing the generation of poor formation at the end of the external electrode due to plating growth.

[0108] This is because a certain thickness is required to ensure the continuity of the lower region 40 of the lower plating layer 30. However, when a given thickness is formed, plating growth can be promoted if a plating solution that can make the metal particle size fine is used.

[0109] When the particle size of the metal particles constituting the lower region 40 of the lower plating layer 30 is larger than 0.20 μm, the compressive stress on the laminate 12 due to the application of thermal stress increases, and cracks may occur in the laminate 12 due to the compressive stress. On the other hand, when the particle size of the metal particles constituting the upper region 42 of the lower plating layer 30 is smaller than 0.5 μm, the upper region 42 is not formed continuously, and, for example, the moisture resistance reliability of the laminated ceramic capacitor 10 may not be guaranteed.

[0110] The upper plating layer 32 includes a first upper plating layer 32 a and a second upper plating layer 32 b .

[0111] The first upper plating layer 32a is configured to cover the first lower plating layer 30a. Specifically, the first upper plating layer 32a is preferably configured on the first end surface 12e of the surface of the first lower plating layer 30a, and is set to also reach the first main surface 12a and the second main surface 12b of the surface of the first lower plating layer 30a. In addition, the first upper plating layer 32a can also be configured only on the surface of the first lower plating layer 30a configured on the first end surface 12e.

[0112] The second upper plating layer 32b is configured to cover the second lower plating layer 30b. Specifically, the second upper plating layer 32b is preferably configured on the second end surface 12f of the surface of the second lower plating layer 30b, and is set to also reach the first main surface 12a and the second main surface 12b of the surface of the second lower plating layer 30b. In addition, the second upper plating layer 32b can also be configured only on the surface of the second lower plating layer 30b configured on the second end surface 12f.

[0113] In the present embodiment, the upper plating layer 32 is a two-layer structure of a Ni plating layer and a Sn plating layer in this order. The Ni plating layer is provided to cover the surface of the lower plating layer 30, thereby preventing the base electrode layer 26 from being corroded by the solder when the multilayer ceramic capacitor 10 is mounted on the mounting substrate. By forming the Sn plating layer, the wettability of the solder when the multilayer ceramic capacitor 10 is mounted on the mounting substrate can be improved, and the multilayer ceramic capacitor 10 can be easily mounted.

[0114] The thickness of each layer of the upper plating layer 32 is preferably 2 μm or more and 11 μm or less.

[0115] The dimension of the length direction z of the multilayer ceramic capacitor 10 including the stack 12, the first external electrode 24a and the second external electrode 24b is set to L dimension, the dimension of the height direction x of the multilayer ceramic capacitor 10 including the stack 12, the first external electrode 24a and the second external electrode 24b is set to T dimension, and the dimension of the width direction y of the multilayer ceramic capacitor 10 including the stack 12, the first external electrode 24a and the second external electrode 24b is set to W dimension.

[0116] Regarding the dimensions of the multilayer ceramic capacitor 10 , preferably, the L dimension in the longitudinal direction z is 0.10 mm to 10.0 mm, the W dimension in the width direction y is 0.10 mm to 10.0 mm, and the T dimension in the height direction x is 20 μm to 10.0 mm.

[0117] according to Figure 1In the illustrated multilayer ceramic capacitor 10, the lower plating layer 30 is a Cu plating layer, and the particle size of the metal particles constituting the lower region 40 of the lower plating layer 30 is smaller than the particle size of the metal particles constituting the upper region 42. Therefore, the adhesion to the laminated body 12 can be ensured by the base electrode layer 26 formed of a thin film layer, and the particle size of the metal particles constituting the lower region 40 is small, so that the compressive stress of the entire lower plating layer 30 can be reduced. As a result, even when thermal stress is applied, the tensile stress applied to the front end of the lower plating layer 30 can be suppressed, and the occurrence of cracks in the laminated body 12 due to the thermal stress can be suppressed.

[0118] In addition, according to Figure 1 In the illustrated multilayer ceramic capacitor 10, in the upper region 42 of the lower plating layer 30, the particle size of the metal particles constituting the upper region 42 is larger than the particle size of the metal particles constituting the lower region 40, so that the thickness of the lower plating layer 30 can be ensured, and the infiltration of moisture into the laminate 12 can be suppressed. As a result, the deterioration of moisture resistance reliability can also be effectively exerted.

[0119] 2. Modification of the first embodiment

[0120] Hereinafter, various modifications (variants 1 to 3) of the multilayer ceramic capacitor as the multilayer ceramic electronic component involved in the first embodiment are described. In addition, regarding these various modifications, the same reference numerals are marked for the components equivalent to the components of the above-mentioned embodiment, and their detailed descriptions are not repeated.

[0121] (1) First Modification

[0122] First, a multilayer ceramic capacitor 110 as a multilayer ceramic electronic component according to a first modification of the first embodiment will be described. Figure 8 This is a perspective view showing the appearance of a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a first modification of the first embodiment of the present invention. Fig. 9 It is a front view showing a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a first modification of the first embodiment of the present invention. Fig.10 It is a plan view showing a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a first modification of the first embodiment of the present invention. Fig.11 yes Figure 1 The cross-sectional view refers to the line XI-XI. Fig.12 yes Figure 1 The cross-sectional view refers to the line XII-XII. Fig.13 yes Figure 1 A cross-sectional view is concerned along line XIII-XIII.

[0123] In the multilayer ceramic capacitor 110 according to the first modification, Figure 8 As shown, the external electrode 124 is arranged not only on the first end surface 12e and the second end surface 12f, the first main surface 12a and the second main surface 12b, but also on the first side surface 12c and the second side surface 12d.

[0124] In addition, if Fig.13 As shown, the shape of the lead electrode portion of the internal electrode layer 16 is also different.

[0125] like Fig.11 as well as Fig.12 As shown, the internal electrode layer 16 includes a first internal electrode layer 16 a and a second internal electrode layer 16 b. The first internal electrode layer 16 a and the second internal electrode layer 16 b are alternately stacked with the ceramic layer 14 interposed therebetween.

[0126] The first internal electrode layer 16a is disposed on the surface of the ceramic layer 14. The first internal electrode layer 16a includes a first opposing electrode portion 18a opposed to the second internal electrode layer 16b and a first lead electrode portion 20a located on one end side of the first internal electrode layer 16a and extending from the first opposing electrode portion 18a to the first end surface 12e side of the stacked body 12. Fig.13 As shown, the end portion of the first lead electrode portion 20a is led out to and exposed at the first end surface 12e, a portion of the first side surface 12c, and a portion of the second side surface 12d.

[0127] The second internal electrode layer 16b is arranged on a surface of a ceramic layer 14 different from the ceramic layer 14 on which the first internal electrode layer 16a is arranged. The second internal electrode layer 16b has a second opposing electrode portion 18b opposed to the first internal electrode layer 16a and a second lead electrode portion 20b located on one end side of the second internal electrode layer 16b and extending from the second opposing electrode portion 18b to the second end face 12f side of the stacked body 12. Fig.13 As shown, the end portion of the second lead electrode portion 20b is led out to and exposed on the second end surface 12f, a portion of the first side surface 12c, and a portion of the second side surface 12d.

[0128] The external electrode 124 includes a base electrode layer 26 and a plating layer 28 formed to cover the base electrode layer 26 .

[0129] The external electrode 124 includes a first external electrode 124 a and a second external electrode 124 b .

[0130] The first external electrode 124a is disposed on the surface of the first end face 12e, a portion of the first main face 12a, a portion of the second main face 12b, a portion of the first side face 12c, and a portion of the second side face 12d of the stacked body 12. In this case, the first external electrode 124a is electrically connected to the first lead electrode portion 20a of the first internal electrode layer 16a.

[0131] The second external electrode 124b is arranged on the surface of the second end face 12f, a portion of the first main face 12a, a portion of the second main face 12b, a portion of the first side face 12c, and a portion of the second side face 12d of the stacked body 12. In this case, the second external electrode 124b is electrically connected to the second lead electrode portion 20b of the second internal electrode layer 16b.

[0132] Incidentally, of course, the structure of the plating layer 28 of the multilayer ceramic capacitor 110 according to the first modification is the same as the structure of the plating layer 28 of the multilayer ceramic capacitor 10 .

[0133] Thus, the lower plating layer 30 can be formed also on the first lead electrode portion 20a and the second lead electrode portion 20b exposed on the first side surface 12c and the second side surface 12d. As a result, the external electrode 124 can be formed also on the first side surface 12c and the second side surface 12d.

[0134] according to Figure 8 The multilayer ceramic capacitor 110 according to the first modification example shown in FIG. Figure 1 The multilayer ceramic capacitor 10 has the same effect.

[0135] (2) Second Modification

[0136] Next, a multilayer ceramic capacitor 210 as a multilayer ceramic electronic component according to a second modification will be described. Fig.14 1 is a central front cross-sectional view showing a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a second modification of the embodiment of the present invention.

[0137] like Fig.14 As shown, a multilayer ceramic capacitor 210 according to the second modification example includes an external electrode 224 having an L-shape in cross-sectional view.

[0138] The external electrode 224 includes a first external electrode 224 a and a second external electrode 224 b .

[0139] In a multilayer ceramic capacitor 210 as a multilayer ceramic electronic component according to a second modification, Fig.14As shown, the L-shaped first external electrode 224a is disposed on the surface of the first end surface 12e and extends from the first end surface 12e to be disposed on the second main surface 12b. In this case, the first external electrode 224a may be disposed so that a part of it surrounds the first main surface 12a.

[0140] Furthermore, in the laminated ceramic capacitor 210, as Fig.14 As shown, the L-shaped second external electrode 224b is arranged on the surface of the second end surface 12f and extends from the second end surface 12f to be arranged on the second main surface 12b. In this case, the second external electrode 224b may be arranged so that a part of it surrounds the first main surface 12a.

[0141] Therefore, in the multilayer ceramic capacitor 210 , only the second foundation electrode layer 26 a 2 and the fourth foundation electrode layer 26 b 2 are arranged on the second main surface 12 b .

[0142] Alternatively, the first external electrode 224a may be disposed on the surface of the first end surface 12e and extended from the first end surface 12e to be disposed on the first main surface 12a, and the second external electrode 224b may be disposed on the surface of the second end surface 12f and extended from the second end surface 12f to be disposed on the first main surface 12a. In this case, the first external electrode 224a may be disposed so that a portion thereof surrounds the second main surface 12b, and the second external electrode 224b may be disposed so that a portion thereof surrounds the second main surface 12b. In this case, only the first base electrode layer and the third base electrode layer are disposed on the first main surface 12a.

[0143] Incidentally, of course, the structure of the plating layer 28 of the multilayer ceramic capacitor 210 according to the second modification is the same as the structure of the plating layer 28 of the multilayer ceramic capacitor 10 .

[0144] according to Fig.14 The multilayer ceramic capacitor 210 according to the second modification example shown in FIG. Figure 1 The same effect as the multilayer ceramic capacitor 10 is achieved, and the following effects are achieved.

[0145] That is, since the external electrode 224 is not formed on the surface of the first main surface 12a, the thickness of the stacked body 12 can be increased in accordance with the absence of such thickness, and the electrostatic capacitance per unit volume of the stacked ceramic capacitor 210 can be increased. In addition, during mounting, the solder can be prevented from wetting the upper surface (first main surface 12a) of the stacked ceramic capacitor 210, and accordingly, the thickness of the stacked body 12 can be further increased.

[0146] (3) Third Modification

[0147] Next, a multilayer ceramic capacitor 310 as a multilayer ceramic electronic component according to a third modification will be described. Fig.15 1 is a central front cross-sectional view showing a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a third modified example of the embodiment of the present invention.

[0148] like Fig.15 As shown, a multilayer ceramic capacitor 310 according to the third modification example includes an external electrode 324 and a via-connecting portion 44 .

[0149] The external electrode 324 includes a first external electrode 324 a and a second external electrode 324 b .

[0150] In a multilayer ceramic capacitor 310 as a multilayer ceramic electronic component according to a third modification, Fig.15 As shown, the internal electrode layer 16 is not led out to both end surfaces.

[0151] The first internal electrode layer 16a includes a first opposing electrode portion 18a opposed to the second internal electrode layer 16b, and a first lead electrode portion 20a located on one end side of the first internal electrode layer 16a and extending from the first opposing electrode portion 18a toward the first end face 12e side of the laminate 12. In addition, the end of the first lead electrode portion 20a is not led to the first end face 12e.

[0152] The second internal electrode layer 16b includes a second opposing electrode portion 18b opposed to the first internal electrode layer 16a, and a second lead electrode portion 20b located on one end side of the second internal electrode layer 16b and extending from the second opposing electrode portion 18b toward the second end face 12f of the laminate 12. The end of the second lead electrode portion 20b is not led to the second end face 12f.

[0153] Furthermore, in the multilayer ceramic capacitor 310 as the multilayer ceramic electronic component according to the third modification, as shown in FIG. Fig.15 As shown, the first external electrode 324a is disposed only on the second main surface 12b, which is the mounting surface, on the first end surface 12e side. In this case, the first external electrode 324a may be disposed so that a portion of it surrounds the first end surface 12e. In this case, Fig.15 As shown, the first external electrode 324 a and the first lead electrode portion 20 a of the first internal electrode layer 16 a are electrically connected via a via connection portion 44 .

[0154] In addition, in a multilayer ceramic capacitor 310 as a multilayer ceramic electronic component according to a third modification, as shown in FIG. Fig.15As shown, the second external electrode 324b is arranged only on the second main surface 12b which becomes the mounting surface on the second end surface 12f side. In this case, the second external electrode 324b may be arranged so that a part of it surrounds the second end surface 12f. In this case, Fig.15 As shown, the second external electrode 324 b and the second lead electrode portion 20 b of the second internal electrode layer 16 b are electrically connected via a via connection portion 44 .

[0155] In addition, the mounting surface may be set to the first main surface 12a and the second main surface 12b. In this case, the external electrode 324 is arranged on the first main surface 12a and the second main surface 12b on the first end surface 12e side, and further arranged on the first main surface 12a and the second main surface 12b on the second end surface 12f side. At this time, the external electrode 324 may also be arranged so that a part of it surrounds the first end surface 12e and the second end surface 12f. In this case, the internal electrode layer 16 and the external electrode 324 are also electrically connected through the via connection portion 44.

[0156] like Fig.15 As shown, the via-hole connection portion 44 realizes the conduction between the internal electrode layer 16 and the external electrode 324. The via-hole connection portion 44 has a laminate hole 46 that penetrates the laminate 12 and a via-hole connection body 48 that is built into the laminate hole 46 and connected to the external electrode 324. In addition, the first lead electrode portion 20a of the first internal electrode layer 16a is electrically connected to the first external electrode 324a via the via-hole connection body 48. In addition, the second lead electrode portion 20b of the second internal electrode layer 16b is electrically connected to the second external electrode 324b via the via-hole connection body 48.

[0157] In addition, the top view shape of the via hole connection portion 44 is not limited to a circle, and can be any shape that can properly realize the conduction of electricity, such as a rectangle, a polygon, an ellipse, etc. In addition, the length of the via hole connection portion 44 on the first external electrode 324a side and the length of the via hole connection portion 44 on the second external electrode 324b side can be formed to be the same length or different lengths.

[0158] according to Fig.15 The multilayer ceramic capacitor 310 according to the third variation shown in FIG. Figure 1 The same effect as the multilayer ceramic capacitor 10 is achieved, and the following effects are achieved.

[0159] That is, since the external electrode 324 is not formed on the surface of the first main surface 12a, the first end surface 12e, and the second end surface 12f, the thickness of the stacked body 12 can be increased corresponding to the absence of such thickness, and the electrostatic capacitance per unit volume of the stacked ceramic capacitor 310 can be increased. In addition, by reducing the mounting height and eliminating the chamfer (fillet), it is possible to perform narrow adjacent mounting on the mounting substrate.

[0160] As described above, the embodiments of the present invention have been disclosed through the above description, but the present invention is not limited thereto.

[0161] 3. Manufacturing method of laminated ceramic capacitor

[0162] Hereinafter, a method for manufacturing a multilayer ceramic capacitor as an example of the multilayer ceramic electronic component according to the first embodiment will be described.

[0163] First, ceramic green sheets and conductive paste for internal electrodes are prepared. The conductive paste for dielectric sheets and internal electrode layers contains a binder (for example, a known organic binder) and a solvent (for example, a known organic solvent).

[0164] Next, a conductive paste for internal electrodes is printed on the ceramic green sheet in a given pattern by, for example, screen printing or gravure printing, to form an internal electrode pattern. Specifically, a paste containing a conductive material is applied to the ceramic green sheet by the above-mentioned printing method or the like, thereby forming a conductive paste layer. The paste containing a conductive material is, for example, a paste in which an organic binder and an organic solvent are added to metal powder. In addition, a ceramic green sheet for an outer layer on which an internal electrode pattern is not printed is also prepared.

[0165] The laminated sheet is produced using the ceramic green sheets on which the internal electrode patterns are formed. That is, a predetermined number of ceramic green sheets for outer layers on which the internal electrode patterns are not formed are laminated, and ceramic green sheets on which the internal electrode patterns corresponding to the first internal electrode layer 16a and ceramic green sheets on which the internal electrode patterns corresponding to the second internal electrode layer 16b are alternately laminated thereon, and a predetermined number of ceramic green sheets for outer layers on which the internal electrode patterns are not formed are further laminated thereon, thereby producing the laminated sheet.

[0166] Furthermore, the laminated sheets are pressed in the laminating direction by a method such as isostatic pressing to produce a laminated block.

[0167] Next, the stacked block is cut into a given size to cut out the stacked chips. At this time, the corners and ridges of the stacked chips may be rounded by barrel grinding or the like.

[0168] Next, the stacked chips are fired to produce the stacked body 12. The firing temperature depends on the materials of the ceramic and the internal electrodes, but is preferably 900°C or higher and 1400°C or lower.

[0169] Next, a base electrode layer 26 composed of a thin film layer is formed on a portion of the first main surface 12a and a portion of the second main surface 12b of the stacked body 12. The base electrode layer 26 as a thin film layer can be formed by, for example, a sputtering method. In other words, the base electrode layer 26 as a thin film layer is composed of a sputtering electrode. The sputtering electrode can be formed of at least one metal selected from Ni, Cr, Cu, Ti, etc.

[0170] Thereafter, a Cu plating layer as the lower plating layer 30 is formed so as to directly cover the base electrode layer 26 composed of the thin film layer and the first end face 12e and the second end face 12f of the laminate 12 where the base electrode layer 26 is not configured. When forming the lower plating layer 30, electrolytic plating using an electrolytic plating solution to which an additive is added or electroless plating based on a substitution reaction is performed. Here, by changing the plating conditions, a lower region 40 located on the laminate 12 side and an upper region 42 located on the surface of the lower region 40 are formed in the lower plating layer 30. The plating conditions are, for example, the plating solution temperature and the plating solution ion concentration, and in the case of electrolytic plating, the current density. As a result, it is possible to achieve a state in which the particle size of the metal particles constituting the lower region 40 is smaller than the particle size of the metal particles constituting the upper region 42.

[0171] Next, an upper plating layer 32 is formed on the surface of the lower plating layer 30. The upper plating layer 32 contains at least one selected from Cu, Ni, Sn, Ag, Pd, Ag-Pd alloy, Au, etc., and is formed of a single layer or multiple layers. Preferably, the upper plating layer 32 is formed of two layers of a Ni plating layer and a Sn plating layer formed on the Ni plating layer.

[0172] As above, it is possible to produce Figure 1 A multilayer ceramic capacitor 10 is described.

[0173] According to the method for manufacturing the multilayer ceramic capacitor according to the present embodiment described above, the multilayer ceramic capacitor according to the present invention with high quality and high performance can be manufactured.

[0174] B. Second Embodiment

[0175] 1. Multilayer ceramic capacitors

[0176] Next, a multilayer ceramic capacitor according to a second embodiment of the present invention will be described. Fig.16 FIG. 1 is a perspective view showing the appearance of a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a second embodiment of the present invention. Fig.17 yes Fig.16 The cross-sectional view refers to the line XVII-XVII. Fig.18 yes Fig.16 The cross-sectional view refers to the line XVIII-XVIII. Fig.19 yes Fig.16 The cross-sectional view refers to the line XIX-XIX. Fig. 20 yes Fig.16 An exploded perspective view of the stack shown. Fig.21A Show Fig.16 FIG. 1 is a first internal electrode pattern of a multilayer ceramic capacitor shown in FIG. Fig.21B Show Fig.16 FIG. 2 is a second internal electrode pattern of a multilayer ceramic capacitor shown in FIG. Fig. 22 It is a schematic cross-sectional view for explaining the structure of the external electrode according to the present invention. Fig.23 It is a schematic cross-sectional view for explaining the structure of the external electrode according to the present invention.

[0177] The multilayer ceramic capacitor 510 includes a multilayer body 512 and external electrodes 524 and 525 .

[0178] The laminate 512 includes a plurality of ceramic layers 514 and a plurality of internal electrode layers 516. The laminate 512 has a first main surface 512a and a second main surface 512b that are opposite to each other in the height direction x, a first side surface 512c and a second side surface 512d that are opposite to each other in the width direction y that is orthogonal to the height direction x, and a third side surface 512e and a fourth side surface 512f that are opposite to each other in the length direction z that is orthogonal to the height direction x and the width direction y. The first main surface 512a and the second main surface 512b extend along the width direction y and the length direction z, respectively. The first side surface 512c and the second side surface 512d extend along the height direction x and the width direction z, respectively. The third side surface 512e and the fourth side surface 512f extend along the height direction x and the length direction y, respectively. Therefore, the so-called height direction x is the direction connecting the first main surface 512a and the second main surface 512b, the so-called width direction y is the direction connecting the first side surface 512c and the second side surface 512d, and the so-called length direction z is the direction connecting the third side surface 512e and the fourth side surface 512f.

[0179] In addition, the stacked body 512 is preferably rounded at corners and ridges. Here, a corner is a portion where three surfaces of the stacked body 512 intersect, and a ridge is a portion where two surfaces of the stacked body 512 intersect.

[0180] like Fig.17 as well as Fig.18As shown, the stack 512 has, in the height direction x connecting the first main surface 512a and the second main surface 512b to each other: an effective layer portion 515a in which a plurality of internal electrode layers 516 are opposed to each other; a first outer layer portion 515b1 formed by a plurality of ceramic layers 514 located between the first main surface 512a and the internal electrode layer 516 located closest to the first main surface 512a; and a second outer layer portion 515b2 formed by a plurality of ceramic layers 514 located between the second main surface 512b and the internal electrode layer 516 located closest to the second main surface 512b.

[0181] The first outer layer portion 515 b 1 is located on the first main surface 512 a side of the laminate 512 , and is an aggregate of a plurality of ceramic layers 514 located between the first main surface 512 a and the internal electrode layer 516 closest to the first main surface 512 a .

[0182] The second outer layer portion 515 b 2 is located on the second main surface 512 b side of the stacked body 512 , and is an aggregate of a plurality of ceramic layers 514 located between the second main surface 512 b and the internal electrode layer 516 closest to the second main surface 512 b .

[0183] The area sandwiched by the first outer layer 515b1 and the second outer layer 515b2 is the effective layer 515a. The number of stacked ceramic layers 514 is not particularly limited, but preferably includes 15 or more and 70 or less of the first outer layer 515b1 and the second outer layer 515b2. In addition, the thickness of the ceramic layer 514 is preferably 0.4 μm or more and 10 μm or less.

[0184] The thickness of the first outer layer portion 515b1 and the second outer layer portion 515b2 is preferably 3 μm or more and 15 μm or less. The region sandwiched between the two outer layer portions 515b1 and 515b2 is the effective layer portion 515a. That is, the effective layer portion 515a is a region where the internal electrode layer 516 is stacked.

[0185] The ceramic layer 514 can be formed of a dielectric material, for example. As the dielectric material, a dielectric ceramic containing a main component such as BaTiO3, CaTiO3, SrTiO3, CaZnO3, etc. can be used. In addition, a material in which a secondary component such as a Mn compound, an Fe compound, a Cr compound, a Co compound, or a Ni compound is added to these main components can also be used.

[0186] The dimensions of the laminate 512 are not particularly limited, but preferably, the L dimension is 0.43 mm or more and 0.73 mm or less, 0.85≤W / L≤1.0, and the T dimension is 50 μm or more and 90 μm or less.

[0187] like Figures 17 to 20As shown, the internal electrode layer 516 includes a plurality of first internal electrode layers 516 a and a plurality of second internal electrode layers 516 b. The first internal electrode layers 516 a and the second internal electrode layers 516 b are alternately stacked with the ceramic layers 514 interposed therebetween.

[0188] The first internal electrode layer 516a is arranged on the surface of the ceramic layer 514. In addition, the first internal electrode layer 516a has a first opposing electrode portion 518a which is opposite to the first main surface 512a and the second main surface 512b and is opposite to the second internal electrode layer 516b, and is stacked in a direction connecting the first main surface 512a and the second main surface 512b.

[0189] In addition, the second internal electrode layer 516b is arranged on the surface of the ceramic layer 514 different from the ceramic layer 514 on which the first internal electrode layer 516a is arranged. The second internal electrode layer 516b has a second opposing electrode portion 518b opposed to the first main surface 512a and the second main surface 512b, and is stacked in the direction connecting the first main surface 512a and the second main surface 512b.

[0190] like Figures 19 to 21B As shown, the first internal electrode layer 516a is led out to the first side surface 512c and the third side surface 512e of the stacked body 512 through the first lead-out electrode portion 520a, and is led out to the second side surface 512d and the fourth side surface 512f of the stacked body 512 through the second lead-out electrode portion 520b. In addition, the width of the first lead-out electrode portion 520a led out to the first side surface 512c may be substantially equal to the width led out to the third side surface 512e, and the width of the second lead-out electrode portion 520b led out to the second side surface 512d may be substantially equal to the width led out to the fourth side surface 512f.

[0191] That is, the first lead electrode portion 520 a is led out to the third side surface 512 e side of the stacked body 512 , and the second lead electrode portion 520 b is led out to the fourth side surface 512 f side of the stacked body 512 .

[0192] The second internal electrode layer 516b is led out to the first side surface 512c and the fourth side surface 512f of the stacked body 512 through the third lead-out electrode portion 521a, and is led out to the second side surface 512d and the third side surface 512e of the stacked body 512 through the fourth lead-out electrode portion 521b. In addition, the width of the third lead-out electrode portion 521a led out to the first side surface 512c may be substantially equal to the width led out to the fourth side surface 512f, and the width of the fourth lead-out electrode portion 521b led out to the second side surface 512d may be substantially equal to the width led out to the third side surface 512e.

[0193] That is, the third lead electrode portion 521 a is led out to the fourth side surface 512 f side of the stacked body 512 , and the fourth lead electrode portion 521 b is led out to the third side surface 512 e side of the stacked body 512 .

[0194] In addition, preferably, when observing the stacked ceramic capacitor 510 from the stacking direction, the straight line connecting the first lead electrode portion 520a and the second lead electrode portion 520b of the first internal electrode layer 516a intersects the straight line connecting the third lead electrode portion 521a and the fourth lead electrode portion 521b of the second internal electrode layer 516b.

[0195] Furthermore, preferably, in the side surfaces 512c, 512d, 512e, and 512f of the stack 512, the first lead electrode portion 520a of the first internal electrode layer 516a and the fourth lead electrode portion 521b of the second internal electrode layer 516b are led to opposite positions, and the second lead electrode portion 520b of the first internal electrode layer 516a and the third lead electrode portion 521a of the second internal electrode layer 516b are led to opposite positions.

[0196] In addition, if Fig.19 As shown, the stacked body 512 includes a side portion (L gap) 522b of the stacked body 512, and the side portion 522b of the stacked body 512 is formed between one end of the first opposing electrode portion 518a in the length direction z and the third side surface 512e and between the other end of the second opposing electrode portion 518b in the length direction z and the fourth side surface 512f. The average length of the side portion (L gap) 522b of the stacked body 512 in the width direction z is preferably 10 μm or more and 60 μm or less, more preferably 10 μm or more and 30 μm or less, and further preferably 10 μm or more and 20 μm or less.

[0197] Furthermore, if Fig.19 As shown, the stacked body 512 includes a side portion (W gap) 522a of the stacked body 512, and the side portion 522a of the stacked body 512 is formed between one end of the first opposing electrode portion 518a in the width direction y and the first side surface 512c and between the other end of the second opposing electrode portion 518b in the width direction y and the second side surface 512d. The average length of the side portion (W gap) 522a of the stacked body 512 in the length direction y is preferably 10 μm or more and 60 μm or less, more preferably 10 μm or more and 30 μm or less, and further preferably 10 μm or more and 20 μm or less.

[0198] As a material of the internal electrode layer 516, for example, metals such as Ni, Cu, Ag, Pd, and Au, and alloys such as Ag-Pd alloys containing one of these metals can be included. The internal electrode layer 516 may further contain dielectric particles of the same composition system as the ceramic contained in the ceramic layer 514. The number of laminated sheets of the internal electrode layer 516 is preferably 20 or more and 80 or less. The average thickness of the internal electrode layer 516 is preferably 0.2 μm or more and 2.0 μm or less.

[0199] like Figures 16 to 19 As shown, external electrodes 524 and 525 are arranged on the stacked body 512 .

[0200] The external electrode 524 includes a base electrode layer 526 and a plating layer 528 formed to cover the base electrode layer 526 .

[0201] The external electrode 525 includes a base electrode layer 527 and a plating layer 529 formed to cover the base electrode layer 527 .

[0202] The external electrode 524 includes a first external electrode 524 a and a second external electrode 524 b .

[0203] The first external electrode 524a is arranged to cover the first extraction electrode portion 520a on the first side surface 512c and the third side surface 512e and to cover a portion of the first main surface 512a and the second main surface 512b. The first external electrode 524a is electrically connected to the first extraction electrode portion 520a of the first internal electrode layer 516a.

[0204] The second external electrode 524b is arranged to cover the second extraction electrode portion 520b on the second side surface 512d and the fourth side surface 512f and to cover a portion of the first main surface 512a and the second main surface 512b. The second external electrode 524b is electrically connected to the second extraction electrode portion 520b of the first internal electrode layer 516a.

[0205] The external electrode 525 includes a third external electrode 525 a and a fourth external electrode 525 b .

[0206] The third external electrode 525a is arranged to cover the third extraction electrode portion 521a on the first side surface 512c and the fourth side surface 512f and to cover a portion of the first main surface 512a and the second main surface 512b. The third external electrode 525a is electrically connected to the third extraction electrode portion 521a of the second internal electrode layer 516b.

[0207] The fourth external electrode 525b is arranged to cover the fourth extraction electrode portion 521b on the second side surface 512d and the third side surface 512e and to cover a portion of the first main surface 512a and the second main surface 512b. The fourth external electrode 525b is electrically connected to the fourth extraction electrode portion 521b of the second internal electrode layer 516b.

[0208] In the stacked body 512, the first opposing electrode portion 518a of the first internal electrode layer 516a and the second opposing electrode portion 518b of the second internal electrode layer 516b are opposed to each other via the ceramic layer 514, thereby forming an electrostatic capacitor. Therefore, an electrostatic capacitor can be obtained between the first external electrode 524a and the second external electrode 524b connected to the first internal electrode layer 516a and the third external electrode 525a and the fourth external electrode 525b connected to the second internal electrode layer 516b, thereby exhibiting the characteristics of a capacitor.

[0209] The base electrode layer 526 includes a first base electrode layer 526a1, a second base electrode layer 526a2, a third base electrode layer 526b1, and a fourth base electrode layer 526b2. In order to further improve performance, the first base electrode layer 526a1, the second base electrode layer 526a2, the third base electrode layer 526b1, and the fourth base electrode layer 526b2 are formed of a thin film layer including a plurality of thin film electrodes.

[0210] The first foundation electrode layer 526a1 is formed so as to cover a portion of the first main surface 512a at a corner where the first main surface 512a, the first side surface 512c, and the third side surface 512e intersect.

[0211] The second foundation electrode layer 526a2 is formed so as to cover a portion of the second main surface 512b at a corner where the second main surface 512b, the first side surface 512c, and the third side surface 512e intersect.

[0212] The third foundation electrode layer 526 b 1 is formed so as to cover a portion of the first main surface 512 a at a corner where the first main surface 512 a , the second side surface 512 d , and the fourth side surface 512 f intersect.

[0213] The fourth foundation electrode layer 526b2 is formed so as to cover a portion of the second main surface 512b at a corner where the second main surface 512b, the second side surface 512d, and the fourth side surface 512f intersect.

[0214] The base electrode layer 527 includes a fifth base electrode layer 527a1, a sixth base electrode layer 527a2, a seventh base electrode layer 527b1, and an eighth base electrode layer 527b2. In order to further improve performance, the fifth base electrode layer 527a1, the sixth base electrode layer 527a2, the seventh base electrode layer 527b1, and the eighth base electrode layer 527b2 are formed of a thin film layer including a plurality of thin film electrodes.

[0215] The fifth foundation electrode layer 527 a 1 is formed so as to cover a portion of the first main surface 512 a at a corner where the first main surface 512 a , the first side surface 512 c , and the fourth side surface 512 f intersect.

[0216] The sixth foundation electrode layer 527 a 2 is formed so as to cover a portion of the second main surface 512 b at a corner where the second main surface 512 b , the first side surface 512 c , and the fourth side surface 512 f intersect.

[0217] The seventh foundation electrode layer 527 b 1 is formed so as to cover a portion of the first main surface 512 a at a corner where the first main surface 512 a , the second side surface 512 d , and the third side surface 512 e intersect.

[0218] The eighth foundation electrode layer 527 b 2 is formed so as to cover a portion of the second main surface 512 b at a corner where the second main surface 512 b , the second side surface 512 d , and the third side surface 512 e intersect.

[0219] The base electrode layers 526 and 527 formed of thin film layers are preferably formed by a thin film forming method such as sputtering or evaporation. In particular, the base electrode layers 526 and 527 formed of thin film layers are preferably sputtering electrodes formed by sputtering. The electrodes formed by sputtering are described below.

[0220] When the base electrode layers 526 and 527 are formed by sputtering electrodes, it is preferable to directly form the sputtering electrodes on a part of the first main surface 512 a and a part of the second main surface 512 b of the stacked body 512 .

[0221] The base electrode layers 526 and 527 formed by the sputtering electrode contain at least one selected from Ni, Cr, Cu, Ti, and the like.

[0222] The thickness of the sputtering electrode in the height direction x connecting the first main surface 512 a and the second main surface 512 b is preferably 50 nm to 400 nm, and more preferably 50 nm to 130 nm.

[0223] The plating layer 528 includes a first plating layer 528a and a second plating layer 528b.

[0224] The first plating layer 528 a is arranged to cover the first foundation electrode layer 526 a 1 and the second foundation electrode layer 526 a 2 .

[0225] The second plating layer 528b is arranged to cover the third foundation electrode layer 526b1 and the fourth foundation electrode layer 526b2.

[0226] The plating layer 529 includes a third plating layer 529a and a fourth plating layer 529b.

[0227] The third plating layer 529 a is arranged to cover the fifth foundation electrode layer 527 a 1 and the sixth foundation electrode layer 527 a 2 .

[0228] The fourth plating layer 529b is arranged to cover the seventh foundation electrode layer 527b1 and the eighth foundation electrode layer 527b2.

[0229] The plating layer 528 and the plating layer 529 may be formed of a plurality of layers.

[0230] Preferably, the plating layer 528 includes a lower plating layer 530 covering the base electrode layer 526 and an upper plating layer 532 configured to cover the lower plating layer 530. Similarly, the plating layer 529 includes a lower plating layer 531 covering the base electrode layer 527 and an upper plating layer 533 configured to cover the lower plating layer 531.

[0231] Among the plating layers 528, the upper plating layer 532 includes, for example, at least one selected from Ni, Sn, Cu, Ag, Pd, Ag-Pd alloy, Au, etc. Similarly, among the plating layers 529, the upper plating layer 533 includes, for example, at least one selected from Ni, Sn, Cu, Ag, Pd, Ag-Pd alloy, Au, etc.

[0232] The lower plating layer 530 includes a first lower plating layer 530 a and a second lower plating layer 530 b .

[0233] The first lower plating layer 530a is arranged on the first side surface 512c and the third side surface 512e of the laminate 512 where no foundation electrode layer is arranged, and is arranged to cover the first foundation electrode layer 526a1 arranged on the first main surface 512a and the second foundation electrode layer 526a2 arranged on the second main surface 512b.

[0234] The second lower plating layer 530b is arranged on the second side surface 512d and the fourth side surface 512f of the laminate 512 where no foundation electrode layer is arranged, and is arranged to cover the third foundation electrode layer 526b1 arranged on the first main surface 512a and the fourth foundation electrode layer 526b2 arranged on the second main surface 512b.

[0235] The lower plating layer 531 includes a third lower plating layer 531 a and a fourth lower plating layer 531 b .

[0236] The third lower plating layer 531a is arranged on the first side surface 512c and the fourth side surface 512f of the stacked body 512 where no foundation electrode layer is arranged, and is arranged to cover the fifth foundation electrode layer 527a1 arranged on the first main surface 512a and the sixth foundation electrode layer 527a2 arranged on the second main surface 512b.

[0237] The fourth lower plating layer 531b is arranged on the second side surface 512d and the third side surface 512e of the laminate 512 where no foundation electrode layer is arranged, and is arranged to cover the seventh foundation electrode layer 527b1 arranged on the first main surface 512a and the eighth foundation electrode layer 527b2 arranged on the second main surface 512b.

[0238] Thus, the plating thickness can be uniform when forming the plating layers after the second layer (upper plating layers 532 and 533), and the effect of suppressing the variation of the plating thickness of the second layer (upper plating layers 532 and 533) can be obtained.

[0239] In the present embodiment, the metal contained in the lower plating layers 530 and 531 is Cu. Therefore, the lower plating layers 530 and 531 are formed as Cu plating layers. Since the lower plating layers 530 and 531 are formed as Cu plating layers and are provided to cover the surfaces of the base electrode layers 526 and 527, there is an effect of suppressing the infiltration of the plating solution.

[0240] Furthermore, if Fig. 22 As shown, the lower plating layer 530 has a lower region 540 located on the laminated body 512 side and an upper region 542 located between the lower region 540 and the upper plating layer 532 .

[0241] Furthermore, the particle size of the metal particles constituting the Cu plating layer located in the lower layer region 540 is smaller than the particle size of the metal particles constituting the Cu plating layer located in the upper layer region 542 .

[0242] In addition, if Fig.23 As shown, the lower plating layer 531 has a lower region 541 located on the laminated body 512 side and an upper region 543 located between the lower region 541 and the upper plating layer 533 .

[0243] Furthermore, the particle size of the metal particles constituting the Cu plating layer located in the lower region 541 is smaller than the particle size of the metal particles constituting the Cu plating layer located in the upper region 543 .

[0244] In addition, the particle size of the metal particles constituting the Cu plating layer means the maximum particle size in the thickness direction of the Cu plating layer.

[0245] Thus, by making the particle size of the particles constituting the lower region 540 of the lower plating layer 530 smaller than the particle size of the metal particles constituting the Cu plating layer located in the upper region 542, it is possible to reduce the compressive stress of the entire lower plating layer 530. In addition, by making the particle size of the metal particles constituting the lower region 541 of the lower plating layer 531 smaller than the particle size of the metal particles constituting the Cu plating layer located in the upper region 543, it is possible to reduce the compressive stress of the entire lower plating layer 531. As a result, even when thermal stress is applied, the tensile stress applied to the front end of the lower plating layers 530 and 531 can be suppressed, and cracks in the stacked body 512 caused by the thermal stress can be suppressed. Furthermore, by making the particle size of the metal particles constituting the upper region 542 of the lower plating layer 530 larger than the particle size of the metal particles constituting the lower region 540, and making the particle size of the metal particles constituting the upper region 543 of the lower plating layer 531 larger than the particle size of the metal particles constituting the lower region 541, the thickness of the lower plating layers 530 and 531 can be ensured, and the infiltration of moisture into the laminate 512 can be suppressed. As a result, it is possible to reduce the stress caused by the application of thermal stress while maintaining good moisture resistance reliability.

[0246] In addition, in the upper region 542 of the lower plating layer 530, the particle size of the metal particles constituting the upper region 542 is large, and in the upper region 543 of the lower plating layer 531, the particle size of the metal particles constituting the upper region 543 is large, so tensile stress caused by thermal stress may sometimes be generated. However, because the particle size of the metal particles constituting the lower regions 540 and 541 is small, the lower regions 540 and 541 become barrier layers, which can suppress cracks caused by the stress generated in the upper regions 542 and 543.

[0247] The thickness of the lower region 540 of the lower plating layer 530 is preferably smaller than the thickness of the upper region 542 of the lower plating layer 530. In addition, the thickness of the lower region 541 of the lower plating layer 531 is preferably smaller than the thickness of the upper region 543 of the lower plating layer 531. As a result, the compressive stress on the stacked body 512 generated in the lower plating layers 530 and 531 due to the application of the thermal cycle is reduced, and the effect of suppressing the generation of cracks in the stacked body 512 due to the compressive stress can be obtained.

[0248] The thickness of the lower region 540 of the lower plating layer 530 and the thickness of the lower region 541 of the lower plating layer 531 are preferably 0.2 μm or more and 1.0 μm or less. When the thickness of the lower region 540 of the lower plating layer 530 and the thickness of the lower region 541 of the lower plating layer 531 are less than 0.2 μm, the lower regions 540 and 541 formed by Cu plating are not continuously formed, and for example, the moisture resistance reliability of the multilayer ceramic capacitor 510 cannot be guaranteed. On the other hand, when the thickness of the lower region 540 of the lower plating layer 530 and the thickness of the lower region 541 of the lower plating layer 531 are greater than 1.0 μm, there is a case where formation defects at the ends of the external electrodes due to plating growth occur.

[0249] The thickness of the upper region 542 of the lower plating layer 530 and the thickness of the upper region 543 of the lower plating layer 531 are preferably 4.0 μm or more and 8.0 μm or less. When the thickness of the upper region 542 of the lower plating layer 530 and the thickness of the upper region 543 of the lower plating layer 531 are less than 4.0 μm, the upper regions 542 and 543 formed by Cu plating are formed discontinuously, and for example, the moisture resistance reliability of the multilayer ceramic capacitor 510 cannot be guaranteed. On the other hand, when the thickness of the upper region 542 of the lower plating layer 530 and the thickness of the upper region 543 of the lower plating layer 531 are greater than 8.0 μm, the thickness of the base body becomes thinner according to the plating thickness, and the required capacitance and strength cannot be exhibited.

[0250] Preferably, the particle size of the metal particles constituting the lower region 540 of the lower plating layer 530 is 0.20 μm or less, and the particle size of the metal particles constituting the upper region 542 of the lower plating layer 530 is 0.50 μm or more. Preferably, the particle size of the metal particles constituting the lower region 541 of the lower plating layer 531 is 0.20 μm or less, and the particle size of the metal particles constituting the upper region 543 of the lower plating layer 531 is 0.50 μm or more. Thus, due to the stress relaxation effect of the lower regions 540, 541 of the lower plating layers 530, 531, the compressive stress on the stacked body 512 due to the application of thermal stress is reduced, and the generation of cracks in the stacked body 512 due to the compressive stress can be suppressed. Furthermore, the metal particles constituting the upper regions 542 and 543 of the lower plating layers 530 and 531 can achieve an effect of suppressing the occurrence of formation defects at the ends of the external electrodes due to plating growth.

[0251] This is because a certain thickness needs to be formed to ensure the continuity of the lower region 540 of the lower plating layer 530 and the lower region 541 of the lower plating layer 531. However, when a given thickness is formed, if a plating solution that can make the metal particle size small is used, plating growth can be promoted.

[0252] When the particle size of the metal particles constituting the lower region 540 of the lower plating layer 530 and the particle size of the metal particles constituting the lower region 541 of the lower plating layer 531 are larger than 0.20 μm, the compressive stress on the laminate 512 due to the application of thermal stress increases, and cracks in the laminate 512 due to the compressive stress may occur. On the other hand, when the particle size of the metal particles constituting the upper region 542 of the lower plating layer 530 and the particle size of the metal particles constituting the upper region 543 of the lower plating layer 530 are smaller than 0.5 μm, the upper regions 542 and 543 of the lower plating layers 530 and 531 are not continuously formed, and, for example, the moisture resistance reliability of the laminated ceramic capacitor 510 may not be guaranteed.

[0253] The upper plating layer 532 includes a first upper plating layer 532 a and a second upper plating layer 532 b .

[0254] The first upper plating layer 532a is configured to cover the first lower plating layer 530a. Specifically, the first upper plating layer 532a is preferably configured on the first side surface 512c and the third side surface 512e of the surface of the first lower plating layer 530a, and is set to also reach the first main surface 512a and the second main surface 512b of the surface of the first lower plating layer 530a.

[0255] The second upper plating layer 532b is configured to cover the second lower plating layer 530b. Specifically, the second upper plating layer 532b is preferably configured on the second side surface 512d and the fourth side surface 512f of the surface of the second lower plating layer 530b, and is set to also reach the first main surface 512a and the second main surface 512b of the surface of the second lower plating layer 530b.

[0256] The upper plating layer 533 includes a third upper plating layer 533 a and a fourth upper plating layer 533 b .

[0257] The third upper plating layer 533a is configured to cover the third lower plating layer 531a. Specifically, the third upper plating layer 533a is preferably configured on the first side surface 512c and the fourth side surface 512f of the surface of the third lower plating layer 531a, and is set to also reach the first main surface 512a and the second main surface 512b of the surface of the third lower plating layer 531a.

[0258] The fourth upper plating layer 533b is configured to cover the fourth lower plating layer 531b. Specifically, the fourth upper plating layer 533b is preferably configured on the second side surface 512d and the third side surface 512e of the surface of the fourth lower plating layer 531b, and is set to also reach the first main surface 512a and the second main surface 512b of the surface of the fourth lower plating layer 531b.

[0259] In this embodiment, the upper plating layers 532 and 533 are two-layer structures of Ni plating layers and Sn plating layers in this order. The Ni plating layers are provided to cover the surfaces of the lower plating layers 530 and 531, thereby preventing the base electrode layers 526 and 527 from being corroded by the solder when the multilayer ceramic capacitor 510 is mounted on the mounting substrate. By forming the Sn plating layer, the wettability of the solder when the multilayer ceramic capacitor 510 is mounted on the mounting substrate can be improved, and the multilayer ceramic capacitor 510 can be easily mounted.

[0260] The thickness of each of the upper plating layers 532 and 533 is preferably 2 μm or more and 11 μm or less.

[0261] The dimension of the length direction z of the stacked ceramic capacitor 510 including the stacked body 512 and the external electrodes 524 and 525 is set to L dimension, the dimension of the height direction x of the stacked ceramic capacitor 510 including the stacked body 512 and the external electrodes 524 and 525 is set to T dimension, and the dimension of the width direction y of the stacked ceramic capacitor 510 including the stacked body 512 and the external electrodes 524 and 525 is set to W dimension.

[0262] Regarding the dimensions of the multilayer ceramic capacitor 510, preferably, the L dimension in the length direction z is greater than or equal to 0.45 mm and less than or equal to 0.75 mm, the T dimension in the height direction x is greater than or equal to 70 μm and less than or equal to 110.0 mm, and the W dimension in the width direction y satisfies 0.85≤W / L≤1.0.

[0263] exist Fig.16 In the illustrated multilayer ceramic capacitor 510 , the same effects as those of the above-described multilayer ceramic capacitor 10 are achieved.

[0264] 2. Modification of the Second Embodiment

[0265] Next, a multilayer ceramic capacitor according to a modified example of the second embodiment of the present invention will be described. Fig.24A It is an external perspective view of a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a modification of the second embodiment of the present invention. Fig. 24B FIG. 1 is a bottom view of a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component according to a modification of the second embodiment of the present invention. Fig.24A as well as Fig. 24BIn the multilayer ceramic capacitor 510' shown in FIG. Figures 16 to 23 The same components of the illustrated multilayer ceramic capacitor 510 are denoted by the same reference numerals, and description thereof will not be repeated.

[0266] The multilayer ceramic capacitor 510 ′ includes a rectangular parallelepiped multilayer body 512 and external electrodes 524 ′ and 525 ′.

[0267] The external electrode 524 ′ includes a first external electrode 524 a ′ formed to be electrically connected to the first lead electrode portion 518 a of the first internal electrode layer 516 a , and a second external electrode 524 b ′ formed to be electrically connected to the second lead electrode portion 520 b .

[0268] The first external electrode 524a' is arranged to cover the first extraction electrode portion 520a on the first side surface 512c and the third side surface 512e, and to cover a portion of the second main surface 512b. In addition, the second external electrode 524b' is arranged to cover the second extraction electrode portion 520b on the second side surface 512d and the fourth side surface 512f, and to cover a portion of the second main surface 512b.

[0269] The external electrode 525 ′ includes a third external electrode 525 a ′ formed to be electrically connected to the third lead electrode portion 521 a of the second internal electrode layer 516 b , and a fourth external electrode 525 b ′ formed to be electrically connected to the fourth lead electrode portion 521 b .

[0270] The third external electrode 525a' is arranged to cover the third extraction electrode portion 521a on the first side surface 512c and the fourth side surface 512f, and to cover a portion of the second main surface 512b. In addition, the fourth external electrode 525b' is arranged to cover the fourth extraction electrode portion 521b on the second side surface 512d and the third side surface 512e, and to cover a portion of the second main surface 512b.

[0271] The external electrodes 524 ′ and 525 ′ preferably include a base electrode layer and a plating layer in this order from the laminated body 512 side.

[0272] Incidentally, of course, the structure of the plated layers 530 and 531 of the multilayer ceramic capacitor 510 ′ according to the present modification is the same as the structure of the plated layers 530 and 531 of the multilayer ceramic capacitor 510 .

[0273] exist Fig.24A as well as Fig. 24B The multilayer ceramic capacitor 510 ′ shown in the figure achieves the same effects as those of the multilayer ceramic capacitor 510 described above, and also achieves the following effects.

[0274] That is, since the external electrodes 524' and 525' are not formed on the surface of the first main surface 512a, the thickness of the stacked body 512 can be increased in accordance with the absence of such thickness, and the strength of the stacked ceramic capacitor 510' can be improved, and the electrostatic capacitance per unit volume can be increased. In addition, during mounting, it is possible to suppress the solder from wetting the upper surface (first main surface 512a) of the stacked ceramic capacitor 510', and accordingly, the thickness of the stacked body 512 can be further increased.

[0275] 3. Manufacturing method of laminated ceramic capacitor

[0276] Next, a method for manufacturing the multilayer ceramic capacitors 510 and 510 ′ will be described.

[0277] First, ceramic green sheets and conductive paste for internal electrodes are prepared. The ceramic green sheets and conductive paste for internal electrodes contain a binder (for example, a known organic binder) and a solvent (for example, an organic solvent).

[0278] Next, a conductive paste for internal electrodes is printed in a given pattern on the ceramic green sheet by, for example, screen printing or gravure printing to form a conductive paste for internal electrodes. Fig.21A as well as Fig.21B Specifically, a paste containing a conductive material is applied to the ceramic green sheet by the above-mentioned printing method, thereby forming a conductive paste layer. The paste containing a conductive material is, for example, a paste in which an organic binder and an organic solvent are added to metal powder. In addition, regarding the ceramic green sheet, a ceramic green sheet for an outer layer without printing an internal electrode pattern is also prepared.

[0279] Then, a laminated sheet is produced using these ceramic green sheets on which the internal electrode patterns are formed. That is, a predetermined number of ceramic green sheets for outer layers on which the internal electrode patterns are not formed are stacked, and ceramic green sheets on which the internal electrode patterns corresponding to the first internal electrode layer 516a and ceramic green sheets on which the internal electrode patterns corresponding to the second internal electrode layer 516b are alternately stacked thereon, and a predetermined number of ceramic green sheets on which the internal electrode patterns are not formed are further stacked thereon, thereby producing a laminated sheet.

[0280] Furthermore, the laminated sheets are pressed in the laminating direction by a method such as isostatic pressing to produce a laminated block.

[0281] Next, the stacked block is cut into a predetermined size to produce a stacked chip. At this time, the corners and ridges of the stacked chip may be rounded by barrel grinding or the like.

[0282] Next, the stacked chips are fired to produce Fig.25The laminated body 512 shown in FIG. 3 is preferably 900° C. or higher and 1300° C. or lower, although the firing temperature depends on the ceramic and the materials of the internal electrodes.

[0283] At this time, if Fig.25 As shown, the first lead electrode portion 520a of the first internal electrode layer 516a is exposed from the first side surface 512c and the third side surface 512e of the stacked body 512, and the third lead electrode portion 521a of the second internal electrode layer 516b is exposed from the first side surface 512c and the fourth side surface 512f of the stacked body 512. In addition, the second lead electrode portion 520b of the first internal electrode layer 516a is exposed from the second side surface 512d and the fourth side surface 512f of the stacked body 512, and the fourth lead electrode portion 521b of the second internal electrode layer 516b is exposed from the second side surface 512d and the third side surface 512e of the stacked body 512.

[0284] Next, if Fig.26 As shown in FIG. 1 , base electrode layers 526 and 527 composed of thin film electrode layers are formed on a portion of the first main surface 512a and a portion of the second main surface 512b of the stacked body 512. The base electrode layers 526 and 527 as thin film layers can be formed, for example, by sputtering. In other words, the base electrode layer as a thin film layer is composed of a sputtering electrode. The sputtering electrode can be formed of at least one metal selected from Ni, Cr, Cu, Ti, etc.

[0285] When the external electrodes 524 ′ and 525 ′ are not arranged on the first main surface 512 a like the multilayer ceramic capacitor 510 ′, the base electrode layers 526 and 527 are not formed on the first main surface 512 a.

[0286] Thereafter, a Cu plating layer is formed as the first lower plating layer 530a so as to be arranged on the first side surface 512c and the third side surface 512e of the stack 512 where no base electrode layer is arranged, thereby covering the first base electrode layer 526a1 arranged on the first main surface 512a and the second base electrode layer 526a2 arranged on the second main surface 512b, and a Cu plating layer is formed as the second lower plating layer 530b so as to be arranged on the second side surface 512d and the fourth side surface 512f of the stack 512 where no base electrode layer is arranged, thereby covering the third base electrode layer 526b1 arranged on the first main surface 512a and the fourth base electrode layer 526b2 arranged on the second main surface 512b.

[0287] In addition, a Cu plating layer is formed as the third lower plating layer 531a so as to be arranged on the first side surface 512c and the fourth side surface 512f of the stack 512 where no base electrode layer is arranged, thereby covering the fifth base electrode layer 527a1 arranged on the first main surface 512a and the sixth base electrode layer 527a2 arranged on the second main surface 512b, and a Cu plating layer is formed as the fourth lower plating layer 531b so as to be arranged on the second side surface 512d and the third side surface 512e of the stack 512 where no base electrode layer is arranged, thereby covering the seventh base electrode layer 527b1 arranged on the first main surface 512a and the eighth base electrode layer 527b2 arranged on the second main surface 512b.

[0288] When forming the lower plating layers 530a, 530b, 531a, 531b, electrolytic plating using an electrolytic plating solution to which an additive is added or electroless plating based on a substitution reaction is performed. Here, by changing the plating conditions, lower regions 540, 541 located on the side of the stack 512 and upper regions 542, 543 located on the surface of the lower regions 540, 541 are formed in the lower plating layers 530a, 530b, 531a, 531b. The plating conditions are, for example, the plating solution temperature and the plating solution ion concentration, and in the case of electrolytic plating, the current density. As a result, it is possible to achieve a state in which the particle size of the metal particles constituting the lower regions 540, 541 is smaller than the particle size of the metal particles constituting the upper regions 542, 543.

[0289] Next, an upper plating layer 532 is formed on the surface of the lower plating layer 530, and an upper plating layer 533 is formed on the surface of the lower plating layer 531. The upper plating layers 532 and 533 contain at least one selected from Cu, Ni, Sn, Ag, Pd, Ag-Pd alloy, Au, etc., and are formed of a single layer or multiple layers. Preferably, the upper plating layers 532 and 533 are formed of two layers, namely, a Ni plating layer and a Sn plating layer formed on the Ni plating layer.

[0290] In this way, Fig. 27 As shown, external electrodes 524 and 525 are formed.

[0291] As above, it is possible to produce Fig.16 or Fig.23 The stacked ceramic capacitors 510, 510' are shown.

[0292] C. Experimental Examples

[0293] Hereinafter, experimental examples of the present invention will be described in detail. Note that these experimental examples do not limit the present invention in any way.

[0294] According to the above-mentioned manufacturing method, a laminated ceramic capacitor was produced as a laminated ceramic electronic component, and the continuity was confirmed by appearance inspection after forming the lower plating layer. In addition, the evaluation was performed by a thermal shock cycle test in the state where the upper plating layer was formed.

[0295] 1. Samples in the Experimental Examples

[0296] In the experimental example, samples with sample numbers 1 to 24 were prepared as samples.

[0297] For each sample, a sample in which the particle diameter of each of the metal particles constituting the lower layer region and the upper layer region in the lower plating layer was changed, and a sample in which the thickness of each of the lower layer region and the upper layer region was changed were prepared.

[0298] The structure of each sample is as follows Figure 1 The stacked ceramic capacitor shown.

[0299] Using the manufacturing method involved in the above embodiment Figure 1 A multilayer ceramic capacitor having the following specifications was produced using the structure shown.

[0300] Dimensions of multilayer ceramic capacitors: L×W×T=0.6mm×0.3mm×0.08mm

[0301] Main component of ceramic layer material: BaTiO3

[0302] Internal electrode material: Ni

[0303] ·External electrode structure

[0304] Base electrode layer: The base electrode layer mainly composed of Ni / Cr alloy is formed by sputtering. Figure 4 As shown, it is assumed that the first end surface and the second end surface of the laminate are not formed on a part of the first main surface and a part of the second main surface, and on a corner portion.

[0305] Plating layer structure

[0306] Lower plating layer: formed by Cu plating. The lower plating layer is formed on the base electrode layer and formed on the first end surface and the second end surface.

[0307] The thickness of the lower layer region is set to be in the range of 0.1 μm or more and 6.0 μm or less.

[0308] The particle size of the metal particles constituting the lower layer region is set to be in the range of 0.05 μm or more and 2.0 μm or less.

[0309] Thickness of the upper layer region: set to be in the range of 1.0 μm or more and 10 μm or less.

[0310] The particle size of the metal particles constituting the upper region is set to be in the range of 0.2 μm or more and 2.0 μm or less.

[0311] Upper plating layer: formed of two layers, a Ni plating layer and a Sn plating layer, from the laminated body side.

[0312] 2. Evaluation Method

[0313] (1) Confirmation of the continuity of the lower plating layer

[0314] Regarding the confirmation of continuity based on the appearance inspection after the lower plating layer is formed, after the lower plating layer is formed, the first end face and the second end face are observed with a microscope, and the state where the lower plating layer is discontinuous and the ceramic layer or the internal electrode is exposed is set as NG. Regarding the number of samples confirmed, each sample number is set to 100, the number of samples judged to be discontinuous is counted, and the defective rate is calculated.

[0315] (2) Thermal shock cycle test

[0316] Regarding the thermal shock cycle test, after forming the upper plating layer, the given evaluation substrate is reflowed with solder and installed, and the temperature in the tank is changed between -55°C and 85°C at intervals of 30 minutes. The change from -55°C to 85°C is set as one cycle, and it is implemented for 200 cycles, and then each sample is grinded from the LT direction for each substrate to expose the cross section. Then, the exposed cross section is observed under a microscope, and the state in which cracks are generated in the laminate is set as NG. Regarding the number of samples tested, each sample number is set to 100, the number of samples judged to have cracks is counted, and the defective rate is calculated. In addition, samples with a defective rate of less than 5% are judged to be good.

[0317] 3. Experimental results

[0318] Tables 1 and 2 show the results of the above experiments.

[0319] [Table 1]

[0320]

[0321] [Table 2]

[0322]

[0323] First, the results of focusing on the relationship between the particle diameter of the metal particles constituting the lower layer region and the particle diameter of the metal particles constituting the upper layer region will be described.

[0324] For each of Sample Nos. 1 to 8 and Sample Nos. 15 to 24, the particle size of the metal particles constituting the lower layer region is smaller than the particle size of the metal particles constituting the upper layer region, and therefore the results of the thermal shock cycle test are good.

[0325] If an attempt is made to compare samples No. 3 to No. 6 and samples No. 20 to No. 24 (in these samples, the thickness of the lower layer region is 0.5 μm), the results of the thermal shock cycle test and the continuity of the lower layer plating layer of each sample No. 3 to No. 5 are good because the particle size of the metal particles constituting the lower layer region is less than 0.2 μm.

[0326] In addition, since the particle diameter of the metal particles constituting the upper layer region of Sample Nos. 20 to 22 was 0.5 μm or more, the results of the thermal shock cycle test and the continuity of the lower plating layer were all good.

[0327] In addition, in Sample Nos. 6 and 8, since the particle diameter of the metal particles constituting the lower layer region was 0.5 μm, the result of the thermal shock cycle test was that the defect rate was 2.0%.

[0328] On the other hand, for each of the samples No. 9 to No. 14, since the particle size of the metal particles constituting the lower region is the same as the particle size of the metal particles constituting the upper region, or the particle size of the metal particles constituting the lower region is larger than the particle size of the metal particles constituting the upper region, the results of the thermal shock cycle test are that any of the samples is more than 7%, which is defective.

[0329] Next, the results of focusing on the relationship between the thickness of the lower layer region and the thickness of the upper layer region will be described.

[0330] Since the thickness of the lower layer region of each of the samples No. 1 to No. 8, No. 17, and No. 20 to No. 24 was smaller than the thickness of the upper layer region, the results of the heat shock cycle test were good.

[0331] In addition, since the particle size of the metal particles constituting the lower layer region of Sample No. 2 to Sample No. 5, Sample No. 7, Sample No. 15, Sample No. 17, and Sample No. 20 to Sample No. 22 is smaller than the particle size of the metal particles constituting the upper layer region, and the thickness of the lower layer region is greater than 0.2 μm and less than 1.0 μm, and the thickness of the upper layer region is greater than 4.0 μm and less than 8.0 μm, the results of the thermal shock cycle test and the continuity of the lower plating layer are both good.

[0332] On the other hand, since the thickness of the lower layer region of sample No. 1 is 0.1 μm, although the result of the thermal shock cycle test is good, the defect rate of the continuity of the lower plating layer is as high as 70%. In addition, since the thickness of the upper layer region of sample No. 16 is 10 μm, the result of the thermal shock cycle test is 5.0%.

[0333] Furthermore, if an attempt is made to compare sample numbers 5, 7, 17 to 19 (in these samples, the particle size of the metal particles constituting the lower layer region is 0.2 μm), the results of the thermal shock cycle test and the continuity of the lower layer plating layer of sample numbers 5, 7 and 17 are all good because the thickness of the lower layer region is smaller than that of the upper layer region.

[0334] On the other hand, in the sample No. 18, since the thickness of the lower layer area is the same as the thickness of the upper layer area, although the result of the thermal shock cycle test is good, the defective rate of the continuity of the lower plating layer is as high as 70%. In the sample No. 19, since the thickness of the lower layer area is larger than the thickness of the upper layer area, the result of the thermal shock cycle test is 3.0%.

[0335] According to the above, in the samples of each sample number, when the particle size of the metal particles constituting the lower layer region is smaller than the particle size of the metal particles constituting the upper layer region, the adhesion to the laminate can be ensured by the base electrode layer formed by the thin film layer, and the particle size of the metal particles constituting the lower layer region is small, so that the compressive stress of the entire lower plating layer can be reduced. As a result, it was confirmed that even when thermal stress is applied, the tensile stress applied to the front end of the lower plating layer can be suppressed, and cracks in the laminate caused by thermal stress can be suppressed.

[0336] For example, although only a shape that is bilaterally symmetrical in the front view is illustrated in the above-mentioned embodiment and each modified example, the outer shape of the laminated ceramic electronic component according to the present invention can be variously changed according to the object to be installed and the performance pursued. In addition, the present invention also includes an embodiment in which all or part of the structures of the above-mentioned embodiment and each modified example are appropriately combined.

[0337] Although the embodiments of the present invention have been described, the embodiments disclosed this time should be considered to be illustrative in all aspects and not restrictive. The scope of the present invention is indicated by the claims, and is intended to include all modifications within the meaning and scope equivalent to the claims.

Claims

1. A laminated ceramic electronic component comprising: A laminated body comprising a plurality of laminated ceramic layers, and having a first main surface and a second main surface opposite to each other in a height direction, a first side surface and a second side surface opposite to each other in a width direction perpendicular to the height direction, and a first end surface and a second end surface opposite to each other in a length direction perpendicular to the height direction and the width direction; a first internal electrode layer, disposed on the ceramic layer and exposed at the first end surface; a second internal electrode layer disposed on the ceramic layer and exposed at the second end surface; a first external electrode connected to the first internal electrode layer and disposed on the first end surface; and a second external electrode connected to the second internal electrode layer and arranged on the second end surface; in, The first external electrode and the second external electrode include: a base electrode layer; a lower plating layer disposed on the first end surface and the second end surface; and an upper plating layer disposed on the lower plating layer. The base electrode layer is a thin film electrode including at least one selected from Ni, Cr, Cu, and Ti. The lower plating layer is composed of a Cu plating layer, The lower plating layer has a lower region located on the laminated body side and an upper region located between the lower region and the upper plating layer. The metal grain size of the Cu plating layer located in the lower region is smaller than the metal grain size of the Cu plating layer located in the upper region. The metal grain size of the Cu plating layer located in the lower region is 0.2 μm or less, The metal grain size of the Cu plating layer located in the upper layer region is 0.5 μm or more.

2. The multilayer ceramic electronic component according to claim 1, wherein The thickness of the lower layer region is smaller than the thickness of the upper layer region.

3. The multilayer ceramic electronic component according to claim 1 or claim 2, wherein: The thickness of the lower layer region is 0.2 μm or more and 1.0 μm or less, The thickness of the upper layer region is 4.0 μm or more and 8.0 μm or less.

4. A laminated ceramic electronic component comprising: A laminate comprising a plurality of stacked ceramic layers and a plurality of internal electrode layers, and having a first main surface and a second main surface opposite to each other in a height direction, a first side surface and a second side surface opposite to each other in a width direction perpendicular to the height direction, and a third side surface and a fourth side surface opposite to each other in a length direction perpendicular to the height direction and the width direction; and A plurality of external electrodes are arranged on the side surface of the stacked body, in, The plurality of internal electrode layers include a plurality of first internal electrode layers and a plurality of second internal electrode layers, and the plurality of first internal electrode layers and the plurality of second internal electrode layers are alternately stacked with the ceramic layers interposed therebetween. The first internal electrode layer comprises: a first lead-out electrode portion led out to one of the first side surface, the second side surface, the third side surface, and the fourth side surface; and a second lead-out electrode portion led out to a side surface other than the side surface to which the first lead-out electrode portion is led out, The second internal electrode layer comprises: a third lead electrode portion led out to one of the first side surface, the second side surface, the third side surface and the fourth side surface; and a fourth lead electrode portion led out to a side surface other than the side surface to which the third lead electrode portion is led out, The plurality of external electrodes include: a first external electrode connected to the first lead-out electrode portion; a second external electrode connected to the second lead-out electrode portion; a third external electrode connected to the third lead-out electrode portion; and a fourth external electrode connected to the fourth lead-out electrode portion. The first external electrode, the second external electrode, the third external electrode, and the fourth external electrode include: a base electrode layer; a lower plating layer disposed on at least one of the third side surface and the fourth side surface; and an upper plating layer disposed on the lower plating layer. The base electrode layer is a thin film electrode including at least one selected from Ni, Cr, Cu, and Ti. The lower plating layer is composed of a Cu plating layer, The lower plating layer has a lower region located on the laminated body side and an upper region located between the lower region and the upper plating layer. The metal grain size of the Cu plating layer located in the lower region is smaller than the metal grain size of the Cu plating layer located in the upper region. The metal grain size of the Cu plating layer located in the lower region is 0.2 μm or less, The metal grain size of the Cu plating layer located in the upper layer region is 0.5 μm or more.

Citation Information

Patent Citations

  • Ceramic electronic part and its manufacture

    JP1996306580A

  • Laminated electronic component and method for manufacturing the same

    JP2009283597A

  • Embedded device, and printed circuit board having the same

    CN105704925A

  • Manufacturing method of laminated ceramic capacitor

    JP2003217969A