A hyperbranched emulsifier for water-based heavy-duty anticorrosive coating resin and preparation method thereof

By designing a hyperbranched emulsifier with a linear hydrophilic-hyperbranched hydrophilic-linear lipophilic structure, the corrosion resistance and viscosity problems of water-based epoxy resin coatings are solved, achieving more stable emulsions and better anti-corrosion properties.

CN116162248BActive Publication Date: 2024-10-11LUDONG UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211713669.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-10-11
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

Existing water-based epoxy resin coatings have low corrosion resistance, and the emulsion viscosity is high and easy to precipitate, affecting stability.

Method used

Using a hyperbranched emulsifier with a linear hydrophilic-hyperbranched hydrophilic-linear lipophilic structure, through the reaction of polyetheramine, hyperbranched polymer and bisphenol A-type epoxy resin, a highly hydrophilic and Highly lipophilic emulsifier that reduces emulsion viscosity and improves stability.

Benefits of technology

It improves the stability and anti-corrosion properties of the emulsion, reduces the particle size and viscosity of the emulsion, and enhances the flexibility and impact resistance of the coating. It is suitable for heavy-duty anti-corrosion fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 221230095938
    Figure 221230095938
Patent Text Reader

Abstract

The invention discloses a hyperbranched emulsifier for water-based heavy-duty anticorrosive coating resin and a preparation method thereof: polyetheramine, phthalic anhydride and dimethyl sulfoxide are added to a container, the temperature is raised to 25-60°C, the reactor is evacuated and filled with nitrogen three times, and refluxed for 6-12 hours to obtain product A. Product A, hyperbranched polymer and dimethyl sulfoxide are added to a container, the temperature is raised to 100-120°C, the reactor is evacuated and filled with nitrogen three times, and refluxed for 12-16 hours to obtain polyetheramine-hyperbranched polymer. The polyetheramine-hyperbranched polymer, epoxy resin and ethylene glycol propyl ether prepared above are mixed uniformly, the temperature is raised to 60-80°C, the reactor is evacuated and filled with nitrogen three times, and refluxed for 16-24 hours. After the reaction is completed, the solvent is removed to obtain a hyperbranched emulsifier. The present invention prepares a hyperbranched emulsifier with both "linear hydrophilic-hyperbranched hydrophilic-linear lipophilic" characteristics through molecular structure design. The double hydrophilic group and the lipophilic group with a highly similar structure to the epoxy resin can make the emulsifier more hydrophilic, and the lipophilic end can be more closely adsorbed on the surface of the epoxy resin particles, thereby improving the emulsification ability of the emulsifier and the centrifugal stability and storage stability of the epoxy emulsion. The introduction of the hyperbranched structure can solve the problems of high emulsion viscosity and easy precipitation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of epoxy resin emulsifiers, and in particular to a hyperbranched emulsifier for water-based heavy-duty anticorrosive coating resin and a preparation method thereof. Background Art

[0002] Epoxy resin is a thermosetting resin with good anti-corrosion properties, excellent adhesion, and excellent physical and mechanical properties. Due to its good electrical insulation and strong stability to chemical reagents, it is widely used in the field of heavy-duty anti-corrosion. Most epoxy coatings are solvent-based, which can easily cause environmental pollution during the preparation and use of the coating. The development of water-based epoxy resin coatings is one of the effective ways to solve the problem of solvent pollution. The key to preparing water-based epoxy resin coatings is the water-based nature of the epoxy resin substrate, that is, using aqueous solution instead of organic solvent as the dispersion medium of epoxy resin, which can effectively reduce the harm caused by organic solvents and reduce the volatile emissions of solvents. However, the introduction of hydrophilic groups in the system will reduce the corrosion resistance of water-based epoxy coatings. Therefore, it is of great significance to develop an emulsifier that can be used to prepare heavy-duty anti-corrosion water-based epoxy resins.

[0003] Hyperbranched polymers are branched polymers that are easy to modify. With their multifunctional groups, spherical structures, and intramolecular cavities, they have many functions and advantages. In industrial production, hyperbranched polymers can be used in adhesives, coatings, dyes, cosmetics, etc. Because hyperbranched polymers have a large number of functional groups, they are easy to modify and can be used to prepare polymer emulsifiers with different structures and properties. At the same time, the introduction of branched structures in emulsifiers can reduce the interaction between molecules and reduce the viscosity of the system, providing a strategy and approach for the preparation of low-viscosity, construction-friendly waterborne epoxy resins.

[0004] Polyetheramine is a linear polymer with an amine group at the end, active chemical properties and good hydrophilicity. The structure and characteristics of polyetheramine give it broad application prospects in the field of heavy-duty corrosion protection. The polyether segment of polyetheramine can "migrate" after the epoxy coating is cured, forming a "soft-hard" segment with the rigid benzene ring structure in the epoxy resin, which can further improve the flexibility and impact resistance of the epoxy coating while ensuring a certain strength of the material, thereby improving its anti-corrosion performance.

[0005] The invention prepares a hyperbranched emulsifier having both "linear hydrophilicity-hyperbranched hydrophilicity-linear lipophilicity" through molecular structure design. The double hydrophilic group and the lipophilic group highly similar to the epoxy resin structure can make the emulsifier more hydrophilic, and the lipophilic end can be more closely adsorbed on the surface of the epoxy resin particles, thereby improving the emulsification ability of the emulsifier and the centrifugal stability and storage stability of the epoxy emulsion. The introduction of the hyperbranched structure can solve the problems of high emulsion viscosity and easy precipitation. Summary of the invention

[0006] Technical problem to be solved: To overcome the shortcomings of the prior art, the present invention provides a hyperbranched emulsifier for water-based heavy-duty anti-corrosion coating resin and a preparation method thereof. By introducing hydrophilic groups, hyperbranched hydrophilic groups, and linear lipophilic groups (which are highly similar in structure to the emulsified portion) having a linear structure, the binding ability of the hydrophobic end in the emulsifier micelles is weakened, so that the emulsifier can be more evenly distributed in the aqueous phase, and the particle size of the latex particles can be made smaller and more uniform, thereby reducing the viscosity of the emulsion and improving the stability of the emulsion.

[0007] The technical solution adopted by the present invention to solve the above problems is: a hyperbranched emulsifier for water-based heavy-duty anticorrosive coating resin and a preparation method thereof, characterized in that it comprises the following steps: adding 80 to 100 parts of polyetheramine, 9 to 11 parts of phthalic anhydride, and 10 to 30 mL of dimethyl sulfoxide to a container, stirring and heating to 25 to 60°C, vacuuming the reactor and filling it with nitrogen three times, and reflux for 6 to 12 hours. After the reaction is completed, dimethyl sulfoxide is removed by reduced pressure distillation to obtain a light yellow viscous product A. 100 parts of product A, 20 to 40 parts of hyperbranched polymer, and 10 to 30 mL of dimethyl sulfoxide are added to a container, heated to 100 to 120°C, vacuuming the reactor and filling it with nitrogen three times, and refluxed for 12 to 16 hours to obtain a polyetheramine-hyperbranched polymer. Take 50-70 parts of polyetheramine-hyperbranched polymer, 20-30 parts of bisphenol A epoxy resin, and 10-30 mL of ethylene glycol propyl ether, raise the temperature to 60-80 ° C, evacuate the reactor and fill it with nitrogen three times, reflux for 16-24 hours, and after the reaction is completed, remove the solvent by reduced pressure distillation to obtain a hyperbranched emulsifier.

[0008] The hyperbranched polymer is any one of hyperbranched polyethyleneimine and hyperbranched polyamide-amine or a mixture of two of them; the polyetheramine is any one of polyetheramine M1000, polyetheramine M2000 and polyetheramine M3000 or a mixture of any two or more of them; the bisphenol A type epoxy resin is any one of bisphenol A type epoxy resin E20, bisphenol A type epoxy resin E44 and bisphenol A type epoxy resin E51 or a mixture of any two or more of them; and the solvent is any one of ethylene glycol propyl ether, ethylene glycol methyl ether, ethylene glycol ethyl ether, propylene glycol methyl ether, propylene glycol ethyl ether and propylene glycol propyl ether or a mixture of any two or more of them.

[0009] Compared with the prior art, the present invention has the following beneficial effects:

[0010] (1) The polyether chain segment of polyetheramine is introduced into the hyperbranched emulsifier. On the one hand, the hydrophilicity of the emulsifier can be improved due to the linear hydrophilic functional group of polyetheramine. On the other hand, it can "migrate" after the epoxy coating is cured and form a "soft-hard" chain segment with the rigid benzene ring structure in the epoxy resin. While ensuring that the material has a certain strength, it can further improve the flexibility and impact resistance of the epoxy coating, thereby improving its anti-corrosion performance.

[0011] (2) Hyperbranched polymers have a large number of functional groups, which makes them easy to modify and can be used to prepare polymer emulsifiers with different structures and properties. At the same time, the introduction of branched structures in emulsifiers can reduce the interaction between molecules, thereby reducing the viscosity of epoxy resin emulsions, which is beneficial to actual production operations.

[0012] (3) The lipophilic end is composed of bisphenol A epoxy resin, which is a linear lipophilic structure. Its structure is highly similar to the structure of the emulsified oil phase-epoxy resin, which enables the emulsifier to better act on the surface of the epoxy resin and improve the stability of the emulsion.

[0013] (4) By introducing hydrophilic groups and linear lipophilic groups with a linear-hyperbranched dual structure (which are highly similar to the structure of the emulsified part), the binding ability of the hydrophobic end in the emulsifier micelle can be weakened, allowing the emulsifier to be more evenly distributed in the aqueous phase, reducing the particle size of the emulsion and facilitating the stability of the emulsion. DETAILED DESCRIPTION

[0014] The present invention will be further described below in conjunction with embodiments:

[0015] Example 1

[0016] (1) Add 10 g of polyetheramine, 1.25 g of phthalic anhydride, and 10 mL of dimethyl sulfoxide to a container, stir and heat to 25 °C, evacuate the reactor and fill it with nitrogen three times, and reflux for 6 h. After the reaction is completed, dimethyl sulfoxide is removed by vacuum distillation to obtain a light yellow viscous product A. Add 5 g of product A, 1 g of hyperbranched polymer, and 10 mL of dimethyl sulfoxide to a container, heat to 100 °C, evacuate the reactor and fill it with nitrogen three times, and reflux for 12 h to obtain polyetheramine-hyperbranched polymer. Take 5 g of polyetheramine-hyperbranched polymer, 2 g of bisphenol A epoxy resin E51, and 10 mL of ethylene glycol propyl ether, heat to 60 °C, evacuate the reactor and fill it with nitrogen three times, and reflux for 16 h. After the reaction is completed, remove the solvent by vacuum distillation to obtain a hyperbranched emulsifier.

[0017] (2) Add 0.6 g of hyperbranched emulsifier, 5 g of epoxy resin E20 and 1 g of ethylene glycol propyl ether into a four-necked flask, and install a mechanical stirrer, a reflux condenser, a thermometer and a constant pressure dropping funnel into the four-necked flask. Under slow stirring, raise the system temperature to 70-80 °C, maintain the temperature of the reaction system for 4 h and continue stirring. Then lower the temperature to 55 °C, add 5.6 g of deionized water into the constant pressure dropping funnel and slowly drip into the reaction system. The viscosity of the epoxy resin in the four-necked flask gradually increases and then slowly decreases, that is, the epoxy system changes from oil-in-water to water-in-oil phase inversion. When all the deionized water is added, continue to slowly stir and keep warm for 2 h to obtain a milky white water-based epoxy resin emulsion with a solid content of 50%, marked as 1.

[0018] Example 2

[0019] (1) Add 9 g of polyetheramine, 1 g of phthalic anhydride, and 20 mL of dimethyl sulfoxide to a container, heat to 40 °C while stirring, evacuate the reactor and fill it with nitrogen three times, and reflux for 8 h. After the reaction is completed, dimethyl sulfoxide is removed by vacuum distillation to obtain a light yellow viscous product A. Add 10 g of product A, 3 g of hyperbranched polymer, and 20 mL of dimethyl sulfoxide to a container, heat to 110 °C, evacuate the reactor and fill it with nitrogen three times, and reflux for 14 h to obtain polyetheramine-hyperbranched polymer. Take 12 g of polyetheramine-hyperbranched polymer, 5 g of bisphenol A epoxy resin E44, and 20 mL of ethylene glycol propyl ether, heat to 70 °C, evacuate the reactor and fill it with nitrogen three times, and reflux for 20 h. After the reaction is completed, remove the solvent by vacuum distillation to obtain a hyperbranched emulsifier.

[0020] (2) Add 0.6 g of hyperbranched emulsifier, 5 g of epoxy resin E20 and 1 g of ethylene glycol propyl ether into a four-necked flask, and install a mechanical stirrer, a reflux condenser, a thermometer and a constant pressure dropping funnel into the four-necked flask. Under slow stirring, raise the system temperature to 70-80 °C, maintain the temperature of the reaction system for 4 h and continue stirring. Then lower the temperature to 55 °C, add 5.6 g of deionized water into the constant pressure dropping funnel and slowly drip into the reaction system. The viscosity of the epoxy resin in the four-necked flask gradually increases and then slowly decreases, that is, the epoxy system changes from oil-in-water to water-in-oil phase inversion. When all the deionized water is added, continue to slowly stir and keep warm for 2 h to obtain a milky white water-based epoxy resin emulsion with a solid content of 50%, marked as No. 2.

[0021] Example 3

[0022] (1) Add 10 g of polyetheramine, 1.1 g of phthalic anhydride, and 30 mL of dimethyl sulfoxide to a container, heat to 60 °C while stirring, evacuate the reactor and fill it with nitrogen three times, and reflux for 12 h. After the reaction is completed, dimethyl sulfoxide is removed by vacuum distillation to obtain a light yellow viscous product A. Add 10 g of product A, 4 g of hyperbranched polymer, and 30 mL of dimethyl sulfoxide to a container, heat to 120 °C, evacuate the reactor and fill it with nitrogen three times, and reflux for 16 h to obtain polyetheramine-hyperbranched polymer. Take 7 g of polyetheramine-hyperbranched polymer, 3 g of bisphenol A epoxy resin E20, and 30 mL of ethylene glycol propyl ether, heat to 80 °C, evacuate the reactor and fill it with nitrogen three times, and reflux for 24 h. After the reaction is completed, remove the solvent by vacuum distillation to obtain a hyperbranched emulsifier.

[0023] (2) Add 0.6 g of hyperbranched emulsifier, 5 g of epoxy resin E20 and 1 g of ethylene glycol propyl ether into a four-necked flask, and install a mechanical stirrer, a reflux condenser, a thermometer and a constant pressure dropping funnel into the four-necked flask. Under slow stirring, raise the system temperature to 70-80 °C, maintain the temperature of the reaction system for 4 h and continue stirring. Then lower the temperature to 55 °C, add 5.6 g of deionized water into the constant pressure dropping funnel and slowly drip into the reaction system. The viscosity of the epoxy resin in the four-necked flask gradually increases and then slowly decreases, that is, the epoxy system changes from oil-in-water to water-in-oil phase inversion. When all the deionized water is added, continue to slowly stir and keep warm for 2 h to obtain a milky white water-based epoxy resin emulsion with a solid content of 50%, marked as No. 3. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The anti-corrosion coating prepared with the emulsion in Examples 1-3 of the present invention was sprayed on a steel plate of the same size, and the water resistance test diagram is shown.

[0025] Table 1 Particle size and stability test results

[0026] serial number Particle size / nm Mechanical stability 3-month stability 1 259 Level 1 Unstratified 2 267 Level 1 Unstratified 3 248 Level 1 Unstratified

[0027] The particle size of epoxy emulsion was determined by the following method: 0.1 g epoxy resin emulsion was diluted to 20 mL with distilled water, 1 mL of the diluted emulsion was taken, and the particle size of the emulsion was tested using a nano-laser particle size analyzer and a zata potential analyzer.

[0028] The mechanical stability of the epoxy resin emulsion was determined by the following method: the mechanical stability of the emulsion was compared by the centrifugal stratification method, and the stability of the emulsion was divided into 5 levels according to different centrifugal times at different speeds.

[0029] Level 1: 3500 r / min×30 min, no stratification

[0030] Level 2: 2500 r / min×30 min, no stratification

[0031] Level 3: 1500 r / min×30 min, no stratification

[0032] Level 4: 1500 r / min×20 min, no stratification

[0033] Level 5: 1000 r / min×20 min, no stratification

[0034] The stability of the epoxy resin emulsion is determined by the following method: the emulsion is sealed in a transparent centrifuge tube, placed in a cool place, and the time it takes for the emulsion to show unstable phenomena such as stratification, cross-linking, and demulsification.

[0035] Depend on Figure 1 As can be seen from the data in Table 1, the accelerated line expansion of the sample evaluated by the epoxy resin emulsion prepared by the present invention is within 0.5 mm, which is level 10 according to the ASTM D1654 standard; no large-scale corrosion occurs on the board surface, and the corrosion level can reach level 10; no bubbling occurs; the emulsion does not have unstable phenomena such as stratification, cross-linking, and demulsification, and the mechanical stability reaches level 1; that is, the emulsion has good corrosion resistance and broad application prospects.

[0036] Factors such as the ratio of hydrophilic to lipophilic units, the type of hyperbranched polymer, reaction temperature and reaction time can affect the implementation of the present invention, and the embodiments will not be listed one by one here.

Claims

1. A method for preparing a hyperbranched emulsifier for water-based heavy-duty anticorrosive coating resin, characterized in that The method comprises the following steps: adding 80 to 100 parts of polyetheramine, 9 to 11 parts of phthalic anhydride and 10 to 30 mL of dimethyl sulfoxide into a container, stirring and heating to 25 to 60°C, evacuating the reactor and filling it with nitrogen three times, and reflux for 6 to 12 hours; after the reaction is completed, removing dimethyl sulfoxide by reduced pressure distillation to obtain a light yellow viscous product A; adding 100 parts of product A, 20 to 40 parts of a hyperbranched polymer and 10 to 30 mL of dimethyl sulfoxide into a container, heating to 100 to 120°C, evacuating the reactor and filling it with nitrogen three times, and reflux for 12 to 16 hours to obtain a polyetheramine-hyperbranched polymer; taking 50 to 70 parts of a polyetheramine-hyperbranched polymer, 20 to 30 parts of a bisphenol A epoxy resin, and 10 to 30 mL of dimethyl sulfoxide; and mixing the obtained product A with 100 to 100 mL of a polyetheramine-hyperbranched polymer. mL is selected from any one of ethylene glycol propyl ether, ethylene glycol methyl ether, ethylene glycol ethyl ether, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol propyl ether, or a mixture of any two or more thereof as a solvent and placed in a container, the temperature is raised to 60-80 °C, the reactor is evacuated and filled with nitrogen three times, refluxed for 16-24 h, and after the reaction is completed, the solvent is removed by reduced pressure distillation to obtain a hyperbranched emulsifier.

2. The method for preparing a hyperbranched emulsifier for a water-based heavy-duty anticorrosive coating resin according to claim 1, characterized in that: The hyperbranched polymer is any one of hyperbranched polyethyleneimine and hyperbranched polyamide-amine or a mixture of the two.

3. The method for preparing a hyperbranched emulsifier for a water-based heavy-duty anticorrosive coating resin according to claim 1, characterized in that: The polyetheramine is any one of polyetheramine M1000, polyetheramine M2000 and polyetheramine M3000, or a mixture of any two or more thereof.

4. The method for preparing a hyperbranched emulsifier for a water-based heavy-duty anticorrosive coating resin according to claim 1, characterized in that: The bisphenol A epoxy resin is any one of bisphenol A epoxy resin E20, bisphenol A epoxy resin E44, and bisphenol A epoxy resin E51, or a mixture of any two or more thereof.

Citation Information

Patent Citations

  • Aqueous hyperbranched polymer emulsifier, and applications thereof in preparing water-borne epoxy resin emulsion

    CN105131305A

  • Preparation method of water-based anticorrosive epoxy coating

    CN111171672A

  • Water-based coating composition and method for forming multilayer coating film

    US20120107619A1

  • Preparation method for waterborne Anti-corrosion resin

    WO2015058684A1