A low-carbon dyed modified wool top and preparation method thereof
By using modified kaolin and sodium benzenesulfonate in low-carbon dyeing strips, combined with improved hygroscopicity of polyethylene glycol, the problems of low dyeing efficiency and floating color are solved, and the goals of efficient dyeing and low-carbon environmental protection are achieved.
Patent Information
- Application Number
- CN202211665170.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-22
AI Technical Summary
The dyeing efficiency of existing low-carbon dyeing strips is limited, and floating color is prone to occur after adding solubilizer, which leads to the need for additional water cleaning, which increases production energy consumption and pollution.
Modified kaolin and sodium benzenesulfonate are used as components of the wool bar matrix and dyeing solution. Modified kaolin increases the looseness of the wool bar matrix and the compatibility of the dispersed dye. Sodium benzenesulfonate promotes the uniform diffusion of the dispersed dye and reduces floating color. The phenomenon is improved by polyethylene glycol and the dyeing efficiency is improved.
It improves dyeing efficiency, reduces floating color phenomenon, saves water consumption, reduces production energy consumption, and achieves the goal of low-carbon environmental protection.
Smart Images

Figure BDA0004013163790000041 
Figure BDA0004013163790000071 
Figure BDA0004013163790000081
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of wool top processing, and more specifically, to a low-carbon dyed modified wool top and a preparation method thereof. Background Art
[0002] Dyeing is an important process in textile processing. Various dyes and auxiliaries are needed in the dyeing process of textiles. The operation of dyeing equipment consumes a lot of energy. In addition, the waste generated in the dyeing process causes serious pollution to the environment. At present, with the gradual increase in low-carbon environmental awareness, the low-carbonization of textile dyeing technology has also become an important part of achieving a low-carbon environmental template.
[0003] In the related art, there is a method for preparing low-carbon dyed wool tops, in which disperse dyes slightly soluble in water are made into disperse dye microcapsules, and then the disperse dye microcapsules are mixed with water to obtain a dyeing solution. The microcapsules have selective permeability to water and disperse dyes. When the polyester wool tops are immersed in the dyeing solution, the disperse dyes will diffuse into the polyester wool tops, thereby completing the dyeing. After dyeing using this method, no additional washing is required, which reduces the energy consumption of the equipment and achieves the purpose of reducing carbon emissions.
[0004] With respect to the above-mentioned related technologies, the inventor believes that when dyeing is performed using the methods in the related technologies, the solubility of disperse dyes in water is low, so the dyeing efficiency is limited. However, if a solubilizing agent is added to the dyeing solution, the disperse dyes will accumulate on the surface of the wool top fibers due to the limited diffusion rate of the disperse dyes in the polyester wool tops, causing floating colors. The floating colors need to be washed with water separately, which is not conducive to reducing production energy consumption and achieving low-carbon environmental protection. Summary of the invention
[0005] In the related art, the solubility of disperse dyes in water is low, so the dyeing efficiency is limited. However, if a solubilizer is added to the dyeing solution, floating color will occur. The floating color needs to be washed with water, which is not conducive to reducing production energy consumption and achieving low-carbon environmental protection. In order to improve this defect, the present application provides a low-carbon dyed modified wool top and a preparation method thereof.
[0006] In the first aspect, the present application provides a low-carbon dyed modified wool top, which adopts the following technical solution:
[0007] A low-carbon dyed modified wool top, which is obtained by immersing a wool top substrate in a dyeing solution and then drying it, wherein the dyeing solution comprises the following components in parts by weight: 100-104 parts of water, 2.8-3.2 parts of disperse dye microcapsules, and 6-8 parts of a diffusion aid; the diffusion aid comprises sodium benzenesulfonate, and the wool top substrate is obtained by spinning a polyester melt, wherein the polyester melt contains 6-8%wt of modified kaolin, and the modified kaolin is kaolin with aromatic groups grafted on the surface.
[0008] By adopting the above technical scheme, the present application selects a wool top matrix containing modified kaolin, and adds a diffusion aid sodium benzenesulfonate to the dyeing solution. As a diffusion aid, the main purpose of sodium benzenesulfonate is to promote the uniform diffusion of disperse dyes in the dyeing solution. Disperse dyes contain a large number of aromatic rings in their molecular structure, and sodium benzenesulfonate has good compatibility with disperse dyes, so sodium benzenesulfonate can also increase the solubility of disperse dyes. Modified kaolin increases the looseness of the wool top matrix structure, expands the gap between molecules, and the aromatic groups on the surface of the modified kaolin make the modified kaolin and disperse dyes have good compatibility, thereby reducing the obstruction of the wool top matrix to the diffusion of disperse dyes, and can accelerate the diffusion rate of disperse dyes in the wool top matrix.
[0009] The solution of the present application improves dyeing efficiency while reducing floating color, thereby eliminating the need for an additional cleaning step, saving water in the dyeing process, and being conducive to reducing production energy consumption and achieving low-carbon environmental protection.
[0010] Preferably, the dyeing solution comprises the following components in parts by weight: 101-103 parts of water, 2.9-3.1 parts of disperse dye microcapsules, and 6.5-7.5 parts of diffusion aid.
[0011] By adopting the above technical solution, the raw material ratio of the dyeing liquid is optimized, which helps to improve the dyeing efficiency.
[0012] Preferably, the polyester melt further contains 2-3%wt polyethylene glycol.
[0013] By adopting the above technical solution, polyethylene glycol can improve the hygroscopicity of the wool top matrix, so that the disperse dye molecules dispersed in water can more easily penetrate into the wool top matrix along with the water, which helps to improve the dyeing efficiency.
[0014] Preferably, the disperse dye microcapsules are prepared according to the following method:
[0015] (1) mixing disperse dye, polydopamine and deionized water, performing shear emulsification, and acidifying with an acidifier to obtain a raw material solution;
[0016] (2) The raw material liquid is heated in a constant temperature water bath, and then the encrypted amine resin prepolymer is added to the raw material liquid. After the addition is completed, the temperature is raised to 60-70° C. and the temperature is kept for 2-3 hours. The pH is then adjusted to 8-9 with ammonia water, and then filtered, washed and dried to obtain disperse dye microcapsules.
[0017] By adopting the above technical scheme, the present application prepares disperse dye microcapsules using melamine resin prepolymer as wall material and disperse dye as core material. The wall material formed by melamine resin prepolymer is permeable to water and dissolved disperse dye molecules, and can achieve sustained release of disperse dye molecules.
[0018] Preferably, the diffusion aid further comprises one of biphenyl and biphenyl ether.
[0019] By adopting the above technical solution, biphenyl and biphenyl ether can be dispersed in the dyeing liquid under the action of benzenesulfonic acid, and biphenyl and biphenyl ether can penetrate into the wool top matrix, promoting the swelling of the wool top matrix. After swelling, the distance between the molecular chains of the wool top matrix becomes larger, making it easier for disperse dyes to enter the wool top matrix, which helps to improve dyeing efficiency.
[0020] Preferably, the diffusion aid is prepared by mixing diphenyl ether and sodium benzene sulfonate in a weight ratio of 1:(2.8-3.2).
[0021] By adopting the above technical solution, the dosage ratio of the diffusion aid when it is a mixture of diphenyl ether and sodium benzene sulfonate is optimized, which helps to improve the dyeing efficiency.
[0022] Preferably, the modified kaolin is prepared according to the following method:
[0023] (1) mixing phenyltriethoxysilane, water and ethanol to obtain a silane-modified liquid;
[0024] (2) Mix kaolin and silane modification liquid, heat at 20-25° C. for 1-2 hours, and then filter and dry to obtain modified kaolin.
[0025] By adopting the above technical solution, the present application modifies kaolin with phenyltriethoxysilane, grafts phenyl groups onto the surface of kaolin, and obtains modified kaolin.
[0026] Preferably, in step (2) of preparing the modified kaolin, sodium benzenesulfonate, kaolin and silane modification liquid are mixed.
[0027] By adopting the above technical scheme, the present application adds sodium benzenesulfonate to the silane coupling agent modification system, and the sulfonic acid group of the sodium benzenesulfonate can electrostatically adsorb with the kaolin particles, thereby improving the dispersion performance of the kaolin particles, reducing the agglomeration of the kaolin particles, and helping to increase the phenyl content on the surface of the modified kaolin, thereby improving the compatibility between the modified kaolin and the disperse dye, making it easier for the disperse dye to gather around the modified kaolin, and helping to speed up the dyeing efficiency.
[0028] Preferably, in step (2) of preparing the modified kaolin, the amount of sodium benzenesulfonate used is 2.6-3.0% by weight of the kaolin.
[0029] By adopting the above technical solution, the present application optimizes the dosage range of sodium benzenesulfonate in the method for preparing modified kaolin, improves the compatibility between modified kaolin and disperse dyes, and helps to accelerate dyeing efficiency.
[0030] In a second aspect, the present application provides a method for preparing low-carbon dyed modified wool tops, which adopts the following technical solution.
[0031] A method for preparing low-carbon dyed modified wool tops comprises the following steps:
[0032] (1) spinning a polyester melt to obtain a wool top matrix; mixing water, disperse dye microcapsules and a diffusion aid to obtain a dyeing solution;
[0033] (2) The wool top substrate is immersed in the dyeing liquid, and then pressurized and heated, and the dyeing liquid is kept warm at 130-140° C. After the insulation is completed, the wool top substrate is taken out, and then dried to obtain a low-carbon dyed modified wool top.
[0034] By adopting the above technical solution, the present application first prepares the wool top matrix and the dyeing liquid respectively, then dyes the wool top matrix under pressurized heating conditions, and then obtains the low-carbon dyed modified wool top after drying.
[0035] In summary, this application has the following beneficial effects:
[0036] 1. The present application increases the solubility of disperse dyes in water by using sodium benzenesulfonate, and accelerates the diffusion rate of disperse dyes in the wool matrix by using modified kaolin, thereby improving the dyeing efficiency and reducing the floating color phenomenon, thereby eliminating the need for additional cleaning steps, saving water in the dyeing process, and being conducive to reducing production energy consumption and achieving low-carbon environmental protection.
[0037] 2. In the present application, the polyester melt preferably also contains 2-3%wt polyethylene glycol, which can improve the hygroscopicity of the wool top matrix, making it easier for disperse dye molecules dispersed in water to penetrate into the wool top matrix along with water, thus helping to improve dyeing efficiency. DETAILED DESCRIPTION
[0038] The present application is further described in detail below in conjunction with embodiments, preparation examples and comparative examples. The raw materials involved in the present application can all be obtained commercially.
[0039] Preparation Example of Disperse Dye Microcapsules
[0040] The following is an explanation using Preparation Example 1.
[0041] Preparation Example 1
[0042] In this preparation example, disperse dye microcapsules were prepared according to the following method:
[0043] (1) 2 kg of disperse dye, 1.6 kg of polydopamine, and 20 kg of deionized water were mixed, and the mixture was sheared and emulsified at a rate of 3000 r / min for 20 min, and then the pH was adjusted to 5 using an acidifier to obtain a raw material solution; in this step, the acidifier was an acetic acid solution with a mass fraction of 5%, and the disperse dye was pure CI Disperse Red 73;
[0044] (2) The raw material liquid is heated in a constant temperature water bath at 20° C., and then 2 kg of melamine resin prepolymer Q3 is added dropwise to the raw material liquid. After the addition is completed, the temperature is raised to 65° C. and the temperature is kept for 2 h. The pH is then adjusted to 8.5 with aqueous ammonia, and then filtered, washed and dried to obtain disperse dye microcapsules.
[0045] Preparation example of modified kaolin
[0046] The following is an explanation using Preparation Example 2.
[0047] Preparation Example 2
[0048] In this preparation example, modified kaolin was prepared according to the following method:
[0049] (1) mixing phenyltriethoxysilane, water and ethanol in a weight ratio of 1:8:5 to obtain a silane-modified liquid;
[0050] (2) Kaolin and silane-modified liquid were mixed in a weight ratio of 3:1, and then heated at 22° C. for 1.5 h, and then filtered and dried to obtain modified kaolin.
[0051] Preparation Example 3
[0052] The difference between this preparation example and preparation example 2 is that in step (2) of preparing modified kaolin, sodium benzenesulfonate, kaolin and silane modification liquid are mixed, and the amount of sodium benzenesulfonate used is 2.4% of the weight of kaolin.
[0053] As shown in Table 1, the difference between Preparation Examples 3-7 is that the proportion of the amount of sodium benzenesulfonate used to the weight of kaolin is different.
[0054] Table 1 The proportion of sodium benzenesulfonate used in kaolin weight
[0055]
[0056] Example
[0057] Examples 1-5
[0058] The following description is given by taking Example 1 as an example.
[0059] Example 1
[0060] In this embodiment, the low-carbon dyed modified wool top is prepared according to the following steps:
[0061] (1) Polyethylene terephthalate and the modified kaolin prepared in Preparation Example 2 are mixed and heated to obtain a polyester melt; the polyester melt is subjected to spinning to obtain a wool top matrix; 100 kg of water, 2.8 kg of the disperse dye microcapsules prepared in Preparation Example 1 and 6 kg of a diffusion aid are mixed to obtain a dyeing solution; in this step, the mass fraction of the modified kaolin in the polyester melt is 6%, and the diffusion aid is sodium benzenesulfonate;
[0062] (2) The wool top substrate is immersed in the dyeing liquid at a bath ratio of 30:1, and then pressurized to 0.7 MPa and heated to 130°C. After being kept at 130°C for 25 minutes, the wool top substrate is taken out and dried to obtain a low-carbon dyed modified wool top.
[0063] As shown in Table 2, the difference between Examples 1-5 mainly lies in the different raw material ratios of the dyeing solution.
[0064] Table 2 Ratio of raw materials of dyeing solution
[0065] sample Water / kg Disperse dye microcapsules / kg Diffusion aid / kg Example 1 100 2.8 6 Example 2 101 2.9 6.5 Example 3 102 3.0 7 Example 4 103 3.1 7.5 Example 5 104 3.2 8
[0066] Embodiment 6-7
[0067] As shown in Table 3, the difference between Examples 6-7 and Example 3 is that the content of modified kaolin in the polyester melt is different.
[0068] Table 3 Mass fraction of modified kaolin in polyester melt
[0069] sample Example 3 Example 6 Example 7 Modified kaolin / % 6 7 8
[0070] Example 8
[0071] The difference between this embodiment and embodiment 6 is that the polyester melt is prepared by mixing polyethylene terephthalate, the modified kaolin of preparation example 2 and polyethylene glycol and then heating and melting. The mass fraction of the modified kaolin in the polyester melt is 7%, and the mass fraction of polyethylene glycol (PEG2000) is 1.8%.
[0072] As shown in Table 4, the difference between Examples 8-12 is that the mass fraction of polyethylene glycol in the polyester melt is different.
[0073] Table 4 Mass fraction of polyethylene glycol in polyester melt
[0074] sample Example 8 Example 9 Example 10 Embodiment 11 Example 12 Polyethylene glycol / % 1.8 2.0 2.5 3.0 3.2
[0075] Embodiment 13
[0076] The difference between this embodiment and embodiment 10 is that the diffusion aid is a mixture of biphenyl and sodium benzene sulfonate in a weight ratio of 1:2.7.
[0077] Embodiment 14
[0078] The difference between this embodiment and embodiment 13 is that the diffusion aid is a mixture of diphenyl ether and sodium benzene sulfonate in a weight ratio of 1:2.7.
[0079] As shown in Table 5, the difference between Examples 14-18 is that the weight ratio of diphenyl ether and sodium benzene sulfonate is different.
[0080] Table 5 Weight ratio of diphenyl ether and sodium benzene sulfonate
[0081] sample Embodiment 14 Embodiment 15 Example 16 Embodiment 17 Embodiment 18 Diphenyl ether: sodium benzene sulfonate 1:2.7 1:2.8 1:3.0 1:3.2 1:3.3
[0082] As shown in Table 6, the difference between Examples 19-23 and Example 6 is that the preparation examples of modified kaolin are different.
[0083] Table 6 Preparation example of modified kaolin
[0084] sample Preparation Example Example 6 Preparation Example 2 Embodiment 19 Preparation Example 3 Embodiment 20 Preparation Example 4 Embodiment 21 Preparation Example 5 Embodiment 22 Preparation Example 6 Embodiment 23 Preparation Example 7
[0085] Comparative Example
[0086] Comparative Example 1
[0087] This comparative example provides a low-carbon dyed modified wool top, which is prepared according to the following steps:
[0088] (1) heating polyethylene terephthalate to obtain a polyester melt; spinning the polyester melt to obtain a wool top matrix; mixing 100 kg of water and 2.8 kg of the disperse dye microcapsules of Preparation Example 1 to obtain a dyeing solution;
[0089] (2) The wool top substrate is immersed in the dyeing liquid at a bath ratio of 30:1, and then pressurized to 0.7 MPa and heated to 130°C. After being kept at 130°C for 25 minutes, the wool top substrate is taken out and dried to obtain a low-carbon dyed modified wool top.
[0090] Comparative Example 2
[0091] The difference between this comparative example and comparative example 1 is that in step (2) of preparing the low-carbon dyed modified wool top, the heat preservation time at 130° C. is 40 minutes.
[0092] Comparative Example 3
[0093] The difference between this comparative example and comparative example 1 is that the dyeing liquid is mixed with 100 kg of water, 2.8 kg of disperse dye microcapsules of preparation example 1 and 6 kg of diffusion aid, and the diffusion aid is sodium benzenesulfonate.
[0094] Comparative Example 4
[0095] The difference between this comparative example and Example 3 is that the components of the dyeing solution do not include a diffusion aid.
[0096] Comparative Example 5
[0097] This comparative example is different from Example 3 in that the components of the polyester melt only include polyethylene terephthalate.
[0098] Comparative Example 6
[0099] The difference between this comparative example and comparative example 3 is that the mass fraction of modified kaolin in the polyester melt is 5%.
[0100] Comparative Example 7
[0101] The difference between this comparative example and comparative example 3 is that the mass fraction of modified kaolin in the polyester melt is 9%.
[0102] Comparative Example 8
[0103] The difference between this comparative example and comparative example 1 is that the modified kaolin in the polyester melt is replaced by kaolin.
[0104] Performance testing methods
[0105] The K / S value of the wool strips was tested on an ORINTEX colorimeter CM-3600d, and the ratio of the K / S value of each embodiment and comparative example to the K / S value of comparative example 1 was calculated. The results were recorded as relative color depth, see Table 7.
[0106] After testing, only Comparative Examples 3 and 5 showed floating color, and the results of Comparative Examples 3 and 5 were measured after washing away the floating color.
[0107] Table 7 Relative color depth
[0108]
[0109]
[0110] Combining Examples 1-5 and Comparative Example 1 and Table 7, it can be seen that the relative color depth measured in Examples 1-5 is greater than that in Comparative Example 1, indicating that the present application increases the solubility of disperse dyes while also enhancing the diffusion effect of disperse dyes in the wool top matrix, thereby improving the dyeing efficiency.
[0111] Combining Examples 1-5 and Comparative Example 2 and Table 7, it can be seen that the relative color depth measured in Examples 1-5 is close to that in Comparative Example 2, and Examples 1-5 only need 25 minutes to achieve the dyeing degree of Comparative Example 2 in 40 minutes, indicating that the present application has indeed improved the dyeing efficiency compared with the related art.
[0112] Combining Comparative Example 1 and Comparative Example 3 and Table 7, it can be seen that the relative color depth of Comparative Example 3 has not increased significantly. Combined with the floating color during dyeing of Comparative Example 3, it can be seen that although the sodium benzenesulfonate added in Comparative Example 3 has a solubilizing effect, the wool strips have not fully absorbed the disperse dye, so the floating color occurs.
[0113] Combining Example 3 and Comparative Example 4 with Table 7, it can be seen that when the dyeing solution lacks the diffusion aid sodium benzenesulfonate, the solubility of the disperse dye is limited, so the dyeing efficiency is affected.
[0114] Combining Example 3 and Comparative Example 5 with Table 7, it can be seen that the relative color depth of Comparative Example 5 has not increased significantly, indicating that the polyester melt of Comparative Example 5 lacks modified kaolin, resulting in poor absorption of disperse dyes by the wool top matrix, which affects the diffusion of disperse dyes into the wool top matrix. Disperse dyes gather on the surface of the wool top matrix, and floating color occurs.
[0115] Combining Example 3, Examples 6-7, Comparative Examples 6-7 and Table 7, it can be seen that when the polyester melt contains 6-8%wt of modified kaolin, the dyeing efficiency is high, while the dyeing efficiency is relatively low when the mass fraction of modified kaolin in the polyester melt is lower than 6%. When the mass fraction of modified kaolin in the polyester melt is higher than 8%, further increasing the content of modified kaolin has little effect on improving the dyeing efficiency.
[0116] Combining Example 3 and Comparative Example 8 with Table 7, it can be seen that kaolin alone has limited effect on improving the diffusion rate of disperse dyes, so the relative color depth of Comparative Example 8 is significantly lower than that of Example 3.
[0117] Combining Example 6 and Examples 8-12 with Table 7, it can be seen that when the polyester melt contains 2-3%wt of polyethylene glycol, the polyethylene glycol can fully improve the hygroscopicity of the wool top matrix, making it easier for the disperse dye molecules dispersed in water to penetrate into the wool top matrix with water, thereby improving the dyeing efficiency. When the polyethylene glycol content is lower than 2%wt, the degree of improvement of the dyeing efficiency by polyethylene glycol is low; and when the polyethylene glycol content is higher than 3%wt, the degree of improvement of the dyeing efficiency by further increasing the polyethylene glycol content is limited.
[0118] It can be seen from Example 10, Examples 13-14 and Table 7 that in the dyeing system of the present application, diphenyl ether has a better swelling effect on the wool top matrix. Therefore, when the diffusion aid contains diphenyl ether, the dyeing efficiency is relatively high.
[0119] It can be seen from Examples 14-18 and Table 7 that when the diffusion aid is mixed with diphenyl ether and sodium benzene sulfonate in a weight ratio of 1:(2.8-3.2), the dyeing efficiency is relatively high.
[0120] It can be seen from Example 6, Examples 19-23 and Table 7 that sodium benzenesulfonate improves the dispersibility of kaolin particles, reduces the agglomeration of kaolin particles, promotes the grafting of silane coupling agents on the surface of kaolin, and increases the phenyl content on the surface of modified kaolin. The increase in phenyl content improves the compatibility between modified kaolin and disperse dyes, so disperse dyes are more likely to gather around the modified kaolin, which helps to speed up dyeing efficiency.
[0121] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A low carbon dyed modified wool top, It is characterized in that The low-carbon dyed modified wool top is obtained by immersing a wool top substrate in a dyeing solution and then drying it, wherein the dyeing solution comprises the following components in parts by weight: 100-104 parts of water, 2.8-3.2 parts of disperse dye microcapsules, and 6-8 parts of a diffusion aid; the diffusion aid comprises sodium benzenesulfonate, and the wool top substrate is obtained by spinning a polyester melt, wherein the polyester melt contains 6-8%wt of modified kaolin, and the modified kaolin is kaolin with aromatic groups grafted on the surface; The modified kaolin is prepared according to the following method: (1) mixing phenyltriethoxysilane, water and ethanol to obtain a silane-modified liquid; (2) Sodium benzenesulfonate, kaolin and silane modified liquid are mixed, and then heated at 20-25° C. for 1-2 hours, and then filtered and dried to obtain modified kaolin; in this step, the amount of sodium benzenesulfonate used is 2.6-3.0% of the weight of kaolin.
2. The low-carbon dyed modified wool top according to claim 1, It is characterized in that The dyeing solution comprises the following components in parts by weight: 101-103 parts of water, 2.9-3.1 parts of disperse dye microcapsules, and 6.5-7.5 parts of diffusion aid.
3. The low-carbon dyed modified wool top according to claim 1, It is characterized in that The polyester melt also contains 2-3%wt polyethylene glycol.
4. The low-carbon dyed modified wool top according to claim 1, It is characterized in that The disperse dye microcapsules are prepared according to the following method: (1) Disperse dye, polydopamine and deionized water are mixed and then sheared and emulsified, and then acidified with an acidifier to obtain a raw material solution; (2) The raw material liquid is heated in a constant temperature water bath, and then the encrypted amine resin prepolymer is added to the raw material liquid. After the addition is completed, the temperature is raised to 60-70°C and kept warm for 2-3 hours. The pH is then adjusted to 8-9 with ammonia water, and then filtered, washed and dried to obtain disperse dye microcapsules.
5. The low-carbon dyed modified wool top according to claim 4, It is characterized in that The diffusion aid further comprises one of biphenyl and biphenyl ether.
6. The low-carbon dyed modified wool top according to claim 5, It is characterized in that The diffusion aid is prepared by mixing diphenyl ether and sodium benzene sulfonate in a weight ratio of 1:(2.8-3.2).
7. A method for preparing the low-carbon dyed modified wool top according to any one of claims 1 to 6, It is characterized in that The following steps are involved: (1) spinning a polyester melt to obtain a wool top matrix; mixing water, disperse dye microcapsules and a diffusion aid to obtain a dyeing solution; (2) Immersing the wool top substrate in the dyeing solution, then pressurizing and heating it, and keeping the dyeing solution warm at 130-140° C. After the insulation is completed, taking out the wool top substrate, and then drying it to obtain a low-carbon dyed modified wool top.