A kind of phosphine oxide porous organic polymer and its application

By introducing olefin-based functional monomers into the phosphine oxide catalyst, porous organic polymers are prepared, forming a firm coordination bond between high concentrations of phosphine oxide and metal, the problem of low catalyst activity and loss is solved, and efficient catalyst design is achieved, improving the improvement of The stability and activity of the catalyst are simplified and the industrial production process is simplified.

CN116178609BActive Publication Date: 2024-12-06DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202111421650.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-26
Publication Date
2024-12-06
Estimated Expiration
2041-11-26

AI Technical Summary

Technical Problem

The existing phosphine oxide catalysts are not active enough in catalytic reactions, which are difficult to recover and use, and the active components are easily lost, resulting in the problem of catalyst deactivation.

Method used

By introducing olefin-based functionalized phosphine oxide monomers for polymerization, a porous organic phosphine oxide polymer was prepared as a support to form a catalyst with a multi-stage porous structure, and a solid coordination bond was formed by coordination between metal and phosphine oxide, thereby enhancing the catalyst. stability and activity.

Benefits of technology

It improves the stability and activity of the catalyst, extends the life of the catalyst, solves the problem of active metal loss, simplifies the separation of reactants and catalysts, and reduces industrial production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116178609B_ABST
    Figure CN116178609B_ABST
Patent Text Reader

Abstract

The present invention relates to polymer materials and catalyst preparation technology, belongs to the field of heterogeneous catalysis, and specifically relates to a phosphine oxide porous organic polymer and its synthesis and application. The present invention introduces olefin groups into phosphine oxide organic monomers, and uses the polymerization reaction of olefin groups on monomer molecules to prepare functional polymers with high bulk concentration of phosphine oxide and developed pores. The high concentration of phosphine oxide monomers in the polymer body can be used as ligands to coordinate with metals to form heterogeneous catalysts. After the phosphine oxide monomers are coordinated with metals, hydroxyl groups connected to P can be formed, which can play the role of acidic functional sites, positioning effect groups, or modifiable sites. Thanks to the synergistic effect of ligands and metals in the prepared catalyst, the finally prepared catalyst can catalyze the selective hydrogenation reaction of α, β-unsaturated aldehydes and ketones, oxidation reactions, carbonylation reactions, photocatalytic hydrogenation reactions, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to polymer materials and catalyst preparation technology, and belongs to the field of heterogeneous catalysis, and in particular to a phosphine oxide porous organic polymer and a preparation method and application thereof. Background Art

[0002] Secondary phosphine oxide (SPO) ligands are stronger electron-donating ligands, more stable in air and easier to synthesize than traditional triphenylphosphine ligands. In essence, SPO ligands exist in a balance between pentavalent phosphine oxide and trivalent phosphorous acid. SPO generally tends to exist in the pentavalent phosphorus state, but when coordinated with a metal, it will be converted into the trivalent phosphorous acid state (Formula 1).

[0003]

[0004] This unique property makes SPO have a structure similar to bidentate chelate ligand after coordination with metal. In 2015, Piet WNM van Leeuwen's research group reported that diphenyl SPO can be used as a good stabilizing group to stabilize Au nanoparticles (J.Am.Chem.Soc.2014,136,2520-2528; J.Am.Chem.Soc.2015,137,7718-7727), and the prepared Au nanoparticles have good results for the hydrogenation of aldehydes. This is mainly because after diphenyl SPO is coordinated with Au nanoparticles, O can activate the cracking hydrogen through synergistic action with Au (Formula 2).

[0005]

[0006] After the phosphine oxide monomer coordinates with the metal, a hydroxyl group connected to P can be formed, which can play the role of an acidic functional site (Catal. Sci. Technol. 2011, 1, 401), a positioning effect group (Org. Lett. 2003, 5, 1503), or a modifiable site (Organometallics 2010, 29, 5953), thereby generating a synergistic effect between the ligand and the metal.

[0007] Recently, Nicola Pinna's research group reported that Au11-SPO can be used for photoelectrocatalytic hydrogenation reactions (J.Am.Chem.Soc.2021,143,25,9595–9600). The Au nanoparticles prepared by these beautiful works can be used as catalysts in catalytic reactions, but the catalysts face the problems of insufficient catalytic activity, difficulty in recycling, and loss of active components of the catalyst. How to solve these problems faces great challenges.

[0008] In recent years, the rapid development of POPs materials has provided an opportunity for the heterogeneity and recycling of catalysts. In 2014, our research group worked together with Xiao Fengshou's research group at Zhejiang University (Chem. Commun., 2014, 50, 11844-11847; J. Mol. Catal. A-Chem., 2015, 404, 211-217; React. Kinet. Mech. Cat., 2015, 116 (1), 223-234) to successfully prepare a polymer-supported heterogeneous hydroformylation catalyst. Studies have shown that the Rh active center on the heterogeneous catalyst is in a single-point dispersed state, which gives the catalyst good activity, and the reason for the catalyst's ultra-high stability is the presence of multiple Rh-P coordination bonds. At present, using the core heterogeneous hydroformylation technology developed by our team, a 50,000 t / a ethylene hydroformylation plant for preparing propanal / n-propanol was successfully started up with one-time feeding of the entire process at Ningbo Juhua New Materials Co., Ltd. on August 26, 2020 and has been running smoothly ever since. The quality of the products propanal and n-propanol have reached international premium standards. This technology solves the problems of ligand and active metal component loss that have not been solved in the heterogeneous catalysis process for more than 80 years (Science China 2020-09-18, Page 4, Comprehensive). Summary of the invention

[0009] Inspired by the success of the previous project of this group, in order to solve the above problems, the purpose of the present invention is to provide a phosphine oxide porous organic polymer and a preparation method and application thereof.

[0010] The technical solution of the present invention is:

[0011] A porous organic polymer of phosphine oxide and its application, wherein an olefin-functionalized phosphine oxide monomer is subjected to polymerization reaction initiated by an initiator to obtain a porous organic polymer of phosphine oxide. P in the prepared polymer body coordinates with a metal to prepare a multiphase catalyst with the porous organic polymer of phosphine oxide as a carrier.

[0012] The olefin group is preferably a vinyl group, and the olefin functionalized phosphine oxide (one or more than one of AF) and the synthesis route are one or more of the following:

[0013]

[0014] The phosphine oxide porous organic polymer has a multi-level pore structure and a specific surface area of ​​10 to 3000 m 2 / g, preferably in the range of 30 to 1000 m 2 / g, containing macropores, mesopores and micropores, with a pore volume of 0.1 to 10.0 cm 3 / g, preferably 0.2 to 2.0 cm 3 / g, and the pore size distribution is 0.01 to 100.0 nm, preferably 0.2 to 5.0 nm.

[0015] The specific preparation steps of the phosphine oxide porous organic polymer are as follows:

[0016] a) adding a vinyl functionalized phosphine oxide monomer, with or without a crosslinking agent, and a free radical initiator to a solvent under an inert gas atmosphere at 273 to 473 K, and stirring the mixture for 0.1 to 100 hours to obtain a prepolymer solution, preferably in a stirring time range of 0.1 to 20 hours;

[0017] b) transferring the prepolymer mixed solution obtained in step a) into a synthesis autoclave, and carrying out polymerization reaction by solvent thermal polymerization under an inert gas atmosphere at 273 to 473 K, stirring for 1 to 100 hours to obtain a phosphine-containing organic polymer;

[0018] c) removing the solvent from the phosphine-containing organic polymer obtained in step b) under vacuum at room temperature to obtain an organic polymer having a multi-level pore structure and containing phosphine oxide functional sites.

[0019] The solvent described in step a) is one or more of water, methanol, ethanol, dichloromethane, chloroform, benzene, toluene, xylene or tetrahydrofuran; the crosslinking agent described in step a) is one or more of styrene, divinylbenzene, tris-phenylene, ethylene, propylene or butadiene; the free radical initiator is one or more of tert-butyl hydroperoxide, azobisisobutyronitrile, azobisisoheptylnitrile, cyclohexanone peroxide or dibenzoyl peroxide.

[0020] In step a), when a crosslinking agent is added, the molar ratio of the vinyl functionalized phosphine oxide monomer to the crosslinking agent is 0.01:1 to 10:1, and the molar ratio of the vinyl functionalized phosphine oxide monomer to the free radical initiator is 300:1 to 10:1. Before polymerizing into an organic polymer, the concentration range of the vinyl functionalized phosphine oxide monomer in the solvent is 0.1-100 g / L; the inert gas in steps a) and b) is selected from one or more of Ar, He, N2 and CO2.

[0021] In addition to bulk polymerization, the polymerization method can also be solution polymerization, suspension polymerization and emulsion polymerization. The polymerization operation temperature range is selected to be 273-473K. The polymerization monomer can be selected from one or more of the phosphine ligands described in claim 2. The polymerized phosphine oxide polymer can be used as a carrier of a multiphase catalyst for preparing a catalyst for the selective hydrogenation reaction, oxidation reaction, carbonylation reaction, and photocatalytic hydrogenation reaction of unsaturated aldehydes.

[0022] The preparation method for the selective hydrogenation reaction of unsaturated aldehydes is as follows: an active metal precursor is prepared into an impregnation solution, added to a carrier, and an equal volume impregnation method or an excess solution impregnation method is adopted, and after reduction and drying steps, a catalyst suitable for the hydrogenation reaction of α, β-unsaturated aldehydes is finally prepared.

[0023] The active metal precursor is selected from one or more of Au, Pd, Co, and Ir, wherein the precursor of Au is one or more of AuCl, (dimethyl sulfide) gold chloride (I), triphenylphosphine gold chloride (I), (tetrahydrothiophene) gold chloride (I), AuCl3, and di(trifluoroacetyl) gold (III); the precursor of Pd is Pd(CH3COO)2, Pd(acac)2, PdCl2, Pd(PPh3)4, and PdCl2(CH3CN)2; the precursor of Co is one or more of Co(CH3COO)2, Co(CO)2(acac), Co(acac)2, and CoCl2; the precursor of Ir is The driving body is one or more of Ir(CO)3(acac), Ir(CH3COO)3, Ir(acac)3, and IrCl4, and the metal loading range of the finally prepared catalyst is 0.01-10wt%; the solvent for preparing the impregnation liquid is one or more of water, benzene, toluene, tetrahydrofuran, methanol, ethanol, dichloromethane or chloroform; the impregnation operation temperature is 243-373K; AlLiH4, NaBH4, or H2 calcination reduction method is adopted for catalyst reduction; vacuum drying method is adopted for catalyst drying, the drying operation temperature is 303-403K, and the operating absolute pressure is maintained below 10kPa during drying.

[0024] Reaction principle of the present invention:

[0025] The present invention introduces olefin groups into phosphine oxide organic monomers, and utilizes the polymerization reaction of the olefin groups on the monomer molecules to prepare a functional polymer with high bulk concentration of phosphine oxide and developed pores. The high-concentration phosphine oxide monomer in the polymer body can be used as a ligand to coordinate with a metal to form a multiphase catalyst. After the phosphine oxide monomer coordinates with the metal, a hydroxyl group connected to P can be formed, and the group can play the role of an acidic functional site, a positioning effect group, or a modifiable site. Thanks to the synergistic effect of the ligand and the metal in the prepared catalyst, the finally prepared catalyst can catalyze the selective hydrogenation reaction, oxidation reaction, carbonylation reaction, photocatalytic hydrogenation reaction, etc. of α, β-unsaturated aldehydes.

[0026] The beneficial effects of the present invention are:

[0027] The polymer phosphine oxide prepared by the present invention has high bulk concentration and developed pores, so that the metal active components in the prepared catalyst form a strong coordination bond with the high-concentration exposed P, the metal active components are not easy to lose, the catalyst is given higher stability, the catalyst life is greatly extended, and the problems of catalyst deactivation and active metal loss are fundamentally solved. The active metal components are highly dispersed in the phosphine-containing organic polymer carrier, which greatly improves the utilization efficiency of the metal and the catalyst activity is also greatly improved. The final catalyst is multiphase, different from the homogeneous reaction system, the separation of reactants and products from the catalyst is simple and efficient, and the cost of subsequent industrial production is greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is distyrylphosphine oxide (A monomer in claim 2) 1 H NMR spectrum.

[0029] Figure 2 is distyrylphosphine oxide (A monomer in claim 2) 13 C NMR spectrum.

[0030] Figure 3 is distyrylphosphine oxide (A monomer in claim 2) 31 P NMR spectrum.

[0031] Figure 4 Schematic diagram of typical cross-linking agents L1-L20 used in polymerization.

[0032] Figure 5 This is the physical adsorption diagram of CPOL-1SPO10DVB.

[0033] Figure 6 This is the pore size distribution diagram of CPOL-1SPO10DVB.

[0034] Figure 7 This is the physical adsorption diagram of POL-SPO.

[0035] Figure 8 This is the pore size distribution diagram of POL-SPO. DETAILED DESCRIPTION

[0036] The following examples are provided to better illustrate the present invention, but are not intended to limit the scope of the present invention.

[0037] The synthesis process of olefin functionalized phosphine oxide AF is shown in the following formula:

[0038]

[0039] Specific preparation steps of monomer A: Under argon protection at 273K, 9g of p-chlorostyrene is dissolved in 50ml of 2-methyltetrahydrofuran, stirred evenly and set aside. 1.7g of magnesium chips are put into a flask, the temperature of the flask is raised to 333K, and about 5ml of a mixed solution of p-chlorostyrene and 2-methyltetrahydrofuran is added dropwise. After the Grignard reagent is initiated, the mixed solution is continued to be added dropwise, and the dropping temperature is maintained at 65°C. After the addition is completed, the Grignard reagent solution of p-chlorostyrene is obtained by keeping the temperature for 1 hour. Then the temperature is lowered to 0 degrees Celsius, and 4.5g of diethyl phosphite and 50ml of the mixed solution are added. After the addition is completed, the reaction is continued for 1 hour. 10 ml of saturated NH4Cl solution was added to quench the reaction, and the mixed solution was separated into two layers. The upper oil layer was taken out, and the solvent was distilled off at 60°C to obtain a light yellow oily liquid. 10 ml of n-heptane was added to heat the mixed solvent to 60°C to fully dissolve it, and then cooled to 0°C for recrystallization and drying to obtain 6.05 g of distyrylphosphine oxide (yield of about 73%, the product was confirmed by nuclear magnetic resonance and high-resolution mass spectrometry), attached Figure 1-3 The NMR of distyrylphosphine oxide A is 1 H. 13 C and 31 P spectrum.

[0040] By replacing p-chlorostyrene with the same molar number of m-chlorostyrene, o-chlorostyrene, 4-vinyl-1-chlorocyclohexane, 3-vinyl-1-chlorocyclohexane and 2-vinyl-1-chlorocyclohexane, and keeping the other preparation steps and conditions the same, monomer BF (the product was confirmed by NMR and high-resolution mass spectrometry) can be prepared with yields of 70%, 39%, 55%, 53% and 38%, respectively.

[0041] Example 1

[0042] Preparation of distyrylphosphine oxide porous organic polymer: 5.0 g distyrylphosphine oxide monomer A and 50.0 g crosslinking agent divinylbenzene (attached) were mixed at 298 K and in an inert gas atmosphere. Figure 4 L1) was dissolved in 550.0 ml of tetrahydrofuran solvent, 0.05 g of azobisisobutyronitrile as a free radical initiator was added to the above solution, and stirred for 2 hours to obtain a prepolymer. The prepolymer was transferred to an autoclave and polymerized by solvent thermal polymerization at 373K and in an inert gas atmosphere for 24 hours. After the autoclave was cooled to room temperature, the solvent was vacuum-evacuated at room temperature to obtain a polymer CPOL-1SPO10DVB copolymerized by distyrylphosphine oxide and divinylbenzene, with a yield of 100%. Figure 5 is the N2 physical adsorption curve of CPOL-1SPO10DVB, attached Figure 6 This is the pore size distribution diagram of CPOL-1SPO10DVB.

[0043] Polymer self-supported highly dispersed Au metal catalyst: 21.0 mg of tetrahydrothiophene gold chloride (I) was weighed and dissolved in 10.0 ml of tetrahydrofuran solvent, 1.0 g of the above-prepared CPOL-1SPO10DVB polymer was added, and stirred at 298K for 5 hours. Then 60.7 mg of LiAlH4 powder was added, and stirring was continued for 5 hours under argon atmosphere at 323K. The solvent was vacuum-evacuated at room temperature to obtain a phosphine oxide polymer self-supported highly dispersed Au-based catalyst.

[0044] Example 2

[0045] In Example 2, except that 50.0 g of the crosslinking agent divinylbenzene ( Figure 4 Except for L1), the rest of the synthesis process is the same as that of Example 1. The physical adsorption curve and pore size distribution diagram of the prepared POL-SPO are shown in the attached figure. Figure 7 and attached Figure 8 shown.

[0046] Example 3

[0047] In Example 3, the synthesis process is the same as that of Example 1 except that the same mole number of benzoyl peroxide is weighed to replace the free radical initiator azobisisobutyronitrile during the polymerization.

[0048] Example 4

[0049] In Example 4, the synthesis process was the same as that of Example 1 except that 50.0 ml of tetrahydrofuran solvent was used instead of 100.0 ml of tetrahydrofuran solvent during the polymerization.

[0050] Example 5

[0051] In Example 5, the synthesis process was the same as that of Example 1 except that 100.0 ml of dichloromethane was used instead of 100.0 ml of tetrahydrofuran during the polymerization.

[0052] Example 6

[0053] In Example 6, except that the polymerization temperature of 393 K was used instead of the polymerization temperature of 373 K, the rest of the synthesis process was the same as that of Example 1.

[0054] Example 7

[0055] In Example 7, except that the bulk polymerization method was replaced by the suspension polymerization method, the remaining methods and catalyst synthesis process were the same as those in Example 1.

[0056] Example 8

[0057] In Example 8, except that m-chlorostyrene is used instead of p-chlorostyrene, the rest of the synthesis process is the same as that of Example 1.

[0058] Example 9

[0059] In Example 9, except that the same molar number of palladium acetate is used to replace tetrahydrothiophene gold (I) chloride, the rest of the synthesis process is the same as that of Example 1, and a highly dispersed Pd-based catalyst can be obtained.

[0060] Example 10

[0061] In Example 10, except that the same molar number of cobalt dichloride is used to replace tetrahydrothiophene gold (I) chloride, the rest of the synthesis process is the same as that of Example 1, and a highly dispersed Ir-based catalyst can be obtained.

[0062] Embodiment 11

[0063] In Example 11, except that the same molar number of acetylacetonato dicarbonyl rhodium is used to replace tetrahydrothiophene gold(I) chloride, the rest of the synthesis process is the same as that of Example 1, and a highly dispersed Co-based catalyst can be obtained.

[0064] Example 12

[0065] In Example 12, except that the same molar number of gold (III) chloride was used to replace tetrahydrothiophene gold (I) chloride, the rest of the synthesis process was the same as that of Example 1.

[0066] Example 13

[0067] In Example 13, we prepared SPO-stabilized Au nanoparticle catalysts according to the literature (J. Am. Chem. Soc. 2014, 136, 2520-2528; J. Am. Chem. Soc. 2015, 137, 7718-7727).

[0068] Embodiment 14

[0069] 0.01mmol of the catalyst prepared above (the amount of catalyst added is calculated according to the molar amount of active metal) was placed in a 50mL reactor, 2mmol of citral (CAS No. 5392-40-5) was added as the reactant, 5ml of tetrahydrofuran was added as the reaction solvent, the reactor was replaced with hydrogen 6 times, 4MPa of hydrogen was filled, the reactor was heated to 60°C and reacted for 10 hours. The reactor was cooled in an ice water bath, ethanol was added as an internal standard, and gas chromatography was performed for analysis. The reaction results are listed in Table 1.

[0070] Table 1 Specific surface area of ​​catalysts synthesized in Examples 1-13 and data of citral hydrogenation reaction

[0071]

[0072]

[0073] Embodiment 15

[0074] 5 g of the catalyst prepared in Example 1 was placed in a fixed bed reactor, and a mixture of CO:O2:N2 = 1:20:79 (V / V / V) was introduced, and the gas space velocity was controlled at 20 L gcat. -1 h -1 The reaction was carried out at a reaction temperature of 100°C and a reaction pressure of 0.1MPa. The CO conversion rate of the tail gas tested by gas chromatography was 99.8%. After the reaction was maintained for 100 hours, the CO conversion rate remained at 99.7%.

[0075] Example 16

[0076] 2 g of the catalyst prepared in Example 11 was loaded into a fixed bed reactor, and quartz sand was added at both ends. A reaction mixture (H2:CO=1:1, V / V) was introduced at 240°C, 3 MPa, and a space velocity of 2000 h -1 Conditions, methanol liquid speed 6h -1 The methanol carbonylation reaction was carried out under 40 °C. The liquid product was analyzed by HP-7890N gas chromatography equipped with HP-5 capillary column and FID detector, and n-butanol was used as internal standard. The reaction tail gas was analyzed online by HP-7890N gas chromatography equipped with Porapak-QS column and TCD detector. The reaction results are listed in the table.

[0077] Table 2. Methanol carbonylation performance of catalyst prepared in Example 11

[0078]

Claims

1. A method for preparing a phosphine oxide porous organic polymer, Features: The porous organic polymer of phosphine oxide is prepared by initiating a polymerization reaction of the olefin groups in the phosphine oxide monomer by an initiator. The olefin-functionalized phosphine oxide monomer is one or more of the following structural formulas AF; 。 2. The preparation method according to claim 1, Features: The synthetic routes of the olefin-functionalized phosphine oxide AF are as follows: 。 3. The preparation method according to claim 1, Features: The specific preparation steps of the phosphine oxide porous organic polymer are as follows: a) adding a vinyl functionalized phosphine oxide monomer, with or without a crosslinking agent, and a free radical initiator to a solvent under an inert atmosphere at 273-473 K, and stirring the mixture for 0.1-100 hours to obtain a prepolymer solution; b) transferring the prepolymer mixed solution obtained in step a) into a synthesis autoclave, and carrying out polymerization reaction by solvent thermal polymerization under an inert atmosphere at 273-473 K for 1-100 hours under stirring to obtain a phosphine-containing organic polymer; c) removing the solvent from the phosphine-containing organic polymer obtained in step b) to obtain an organic polymer having a multi-level pore structure and containing phosphine oxide functional sites.

4. The preparation method according to claim 3, Features: The stirring time ranges from 0.1 to 20 hours.

5. The preparation method according to claim 3, Features: The solvent in step a) is one or more of water, methanol, ethanol, dichloromethane, chloroform, benzene, toluene, xylene or tetrahydrofuran; The crosslinking agent in step a) is one or both of divinylbenzene and butadiene; The free radical initiator is one or more of tert-butyl hydroperoxide, azobisisobutyronitrile, azobisisoheptanenitrile, cyclohexanone peroxide or dibenzoyl peroxide.

6. The preparation method according to claim 3 or 4, Features: In step a), when a cross-linking agent is added, the molar ratio of the vinyl functionalized phosphine oxide monomer to the cross-linking agent is 0.01:1 to 10:1, and the molar ratio of the vinyl functionalized phosphine oxide monomer to the free radical initiator is 1000:1 to 10:1; Before polymerizing into an organic polymer, the concentration of the vinyl functionalized phosphine oxide monomer in the solvent is in the range of 0.1-100 g / L; The inert atmosphere gas in steps a) and b) is selected from Ar, He, N 2 and CO 2 One or more of the following.

7. A porous organic polymer of phosphine oxide prepared by the preparation method according to any one of claims 1 to 6.

8. The phosphine oxide porous organic polymer according to claim 7, Features: The phosphine oxide porous organic polymer has a multi-level pore structure and a specific surface area of ​​10-3000 m 2 / g, pore volume is 0.1~10.0cm 3 / g, and the pore size distribution is 0.01~100.0nm.

9. The phosphine oxide porous organic polymer according to claim 8, Features: The phosphine oxide porous organic polymer has a multi-level pore structure and a specific surface area of ​​30 to 1000 m 2 / g, pore volume is 0.2~2.0cm 3 / g, and the pore size distribution is 0.2~5.0nm.

10. Use of the porous organic polymer of phosphine oxide according to claim 7 or 8, wherein the porous organic polymer of phosphine oxide can be used as a carrier to load active metals to prepare a multiphase catalyst, and P in the polymer bulk can coordinate with the active metals.

11. The use according to claim 10, wherein the multiphase catalyst is a catalyst for the selective hydrogenation reaction of citral, the oxidation reaction of carbon monoxide, and the carbonylation reaction of methanol.

Citation Information

Patent Citations

  • Phosphorus-containing catalyst composition and hydroformylation process using the same

    CN101801528A

  • Metal-phosphine-containing organic copolymer catalyst, preparation method of catalyst, and application of catalyst

    CN107790188A

  • Catalyst for preparing linear-chain aldehyde in high-selectivity manner as well as preparation and application thereof

    CN109806911A

  • Methods for producing aldehyde using phosphorus-containing catalyst composition

    KR1020100092169A