Composition for polyethylene material, polyethylene material and preparation method

Through the combination of antioxidants, light stabilizers, ultraviolet absorbers and anionic adsorbents, the modified polyethylene materials are mixed to solve the problems of antibacterial, anti-chlorine and photothermal oxygen aging properties in long-term use. It realizes the efficient anti-ultraviolet and anti-bacterial properties of PE-RT pipes used in water purifiers.

CN116178816BActive Publication Date: 2024-11-12RIFENG ENTERPRISE FOSHAN CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211600194.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-12
Publication Date
2024-11-12
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

In the long-term use of existing polyethylene materials, it is difficult to take into account both antibacterial, chlorine and photothermal oxygen aging properties. Especially in the environment where drinking water is transported, it is susceptible to oxidative damage from chlorine-containing disinfectants and ultraviolet radiation, resulting in a decline in material performance. .

Method used

Using a combination of antioxidants, light stabilizers, ultraviolet absorbers and anionic adsorbents, a polyethylene material that is anti-ultraviolet, antibacterial and chlorine is prepared through blending and modification technology to ensure the long-term photoaging and antibacterial properties of the material. and long-term mechanical properties.

Benefits of technology

It effectively improves the long-term photoaging performance, antibacterial performance, chlorine resistance and long-term mechanical properties of polyethylene materials. It is suitable for PE-RT pipes of water purifiers, ensuring the overall performance and safety of use of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses a composition for polyethylene material, polyethylene material and preparation method, wherein the composition for polyethylene material comprises 0.5-5 parts by weight of antibacterial agent, 0.1-0.5 parts by weight of anion adsorbent, 0.1-0.5 parts by weight of ultraviolet absorber, 0.1-0.5 parts by weight of light stabilizer, 0.1-0.5 parts by weight of primary antioxidant and 0.2-1 parts by weight of auxiliary antioxidant. The present invention uses antioxidant, light stabilizer, ultraviolet absorber and anion adsorbent in combination to perform blending modification on PE-RT material, ensure the long-term light aging performance, antibacterial performance, chlorine resistance and long-term mechanical performance of the material, and prepares anti-ultraviolet, antibacterial and anti-chlorine polyethylene material for PE-RT pipe of water purifier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polyethylene, in particular to a composition for polyethylene material, a polyethylene material and a preparation method thereof. Background Art

[0002] It is particularly important to strengthen antibacterial awareness and expand the application areas of antibacterial materials. As a water transportation medium, pipes need to have enhanced antibacterial functions in particular when it comes to drinking. In the actual use environment of pipes, the water transported may be disinfected with chlorine-containing disinfectants, and the residual chloride ions in the water also have a strong oxidizing effect on the pipes. At the same time, the long-term light, heat and oxygen aging performance of the exposed use of pipes must be taken into account. Therefore, in a PE-RT pipe that can be used to transport drinking water, it is particularly necessary to use anti-ultraviolet, antibacterial and anti-chlorine polyethylene materials to ensure the safety and health of drinking water.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The object of the present invention is to provide a composition for a polyethylene material, a polyethylene material and a preparation method.

[0005] The present invention is achieved in that:

[0006] In a first aspect, the present invention provides a composition for polyethylene materials, comprising 0.5-5 parts by weight of an antibacterial agent, 0.1-0.5 parts by weight of an anion adsorbent, 0.1-0.5 parts by weight of an ultraviolet absorber, 0.1-0.5 parts by weight of a light stabilizer, 0.1-0.5 parts by weight of a primary antioxidant and 0.2-1 parts by weight of a secondary antioxidant.

[0007] In an optional embodiment, the antibacterial agent is one or more of Ag-Cu / SiO2, silver / activated carbon, Ag / ZnO and chitosan.

[0008] In an optional embodiment, the ultraviolet absorber is one or more of 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-[2-hydroxy-5-(1,1,3,3-tetramethylbutyl)phenyl]benzotriazole and 2,2'-methylenebis[6-(2H-benzotriazole-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol].

[0009] In an optional embodiment, the light stabilizer is one or more of bis(2,2,6,6-tetramethylpiperidinyl)sebacate, poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinethanol) succinate and poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediol[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}.

[0010] In an optional embodiment, the primary antioxidant is one or more of 1,3,5-trimethyl-2,4,6-(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid (3114), 2,2'-oxalylamino-bis[ethyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)]propionate, 1,3,5-tris[[4-(1,1-dimethylethyl)-3-hydroxy-2,6-dimethylphenyl]methyl]-1,3,5-triazine-2,4,6-trione and 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane.

[0011] In an optional embodiment, the secondary antioxidant is one or more of dilauryl thiodipropionate, dioctadecyl thiodipropionate, dilauryl thiodipropionate, tris(2,4-di-tert-butylphenyl) phosphite and dioctadecyl pentaerythritol diphosphite.

[0012] In an optional embodiment, the anion adsorbent is one of hydrotalcite or a hydrotalcite-like material and a lignocellulose anion exchanger.

[0013] In an optional embodiment, the light stabilizer includes poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinylethanol) succinate and poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediol[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}; and / or the ultraviolet absorber includes 2-hydroxy-4-n-octyloxybenzophenone and 2-[2-hydroxy-5-(1,1,3,3-tetramethylbutyl)phenyl]benzotriazole.

[0014] In a second aspect, the present invention provides a polyethylene material comprising 93wt%-98wt% of polyethylene and 2wt%-7wt% of the composition for polyethylene material according to any one of the aforementioned embodiments.

[0015] In a third aspect, the present invention provides a method for preparing the polyethylene material described in the aforementioned embodiment, wherein the mixed raw materials are put into a co-rotating twin-screw granulation device for granulation to obtain a modified polyethylene material, wherein the material temperature is 160°C-230°C.

[0016] The present invention has the following beneficial effects:

[0017] The present invention uses an antioxidant, a light stabilizer, an ultraviolet absorber, an antibacterial agent and an anion adsorbent to perform blending modification on the PE-RT material, thereby ensuring the long-term light aging performance, antibacterial performance, chlorine resistance and long-term mechanical properties of the material, and preparing an anti-ultraviolet, antibacterial and anti-chlorine polyethylene material for PE-RT pipes of water purifiers. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0019] The present embodiment provides a composition for polyethylene material, comprising 0.5-5 parts by weight of an antibacterial agent, 0.1-0.5 parts by weight of an anion adsorbent, 0.1-0.5 parts by weight of an ultraviolet absorber, 0.1-0.5 parts by weight of a light stabilizer, 0.1-0.5 parts by weight of a primary antioxidant and 0.2-1 parts by weight of a secondary antioxidant.

[0020] The present invention uses an antioxidant, a light stabilizer, an ultraviolet absorber, an antibacterial agent and an anion adsorbent to perform blending modification on the PE-RT material, thereby ensuring the long-term light aging performance, antibacterial performance, chlorine resistance and long-term mechanical properties of the material, and preparing an anti-ultraviolet, antibacterial and anti-chlorine polyethylene material for PE-RT pipes of water purifiers.

[0021] Specifically, in some embodiments, the antibacterial agent can be 0.1, 0.2, 0.3, 0.4 or 0.5 parts by weight, the anion adsorbent can be 0.1, 0.2, 0.3, 0.4 or 0.5 parts by weight, the ultraviolet absorber can be 0.1, 0.2, 0.3, 0.4 or 0.5 parts by weight, the light stabilizer can be 0.1, 0.2, 0.3, 0.4 or 0.5 parts by weight, the primary antioxidant can be 0.1, 0.2, 0.3, 0.4 or 0.5 parts by weight and the auxiliary antioxidant can be 0.2, 0.4, 0.6, 0.8 or 1.0 parts by weight. Of course, each component can also select any value within the corresponding range.

[0022] In some embodiments of the present application, the antibacterial agent is one or more of Ag-Cu / SiO2, silver / activated carbon, Ag / ZnO and chitosan.

[0023] In this embodiment, Ag-Cu / SiO2 refers to silicon dioxide-coated silver-copper nanoparticles, silver / activated carbon refers to silver-loaded activated carbon, and Ag / ZnO refers to silver-based inorganic antibacterial materials with nano-ZnO as a carrier.

[0024] In some embodiments of the present application, the ultraviolet absorber is one or more of 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-[2-hydroxy-5-(1,1,3,3-tetramethylbutyl)phenyl]benzotriazole and 2,2'-methylenebis[6-(2H-benzotriazole-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol].

[0025] In some embodiments, the ultraviolet absorber selects 2-hydroxy-4-n-octyloxybenzophenone and 2-[2-hydroxy-5-(1,1,3,3-tetramethylbutyl)phenyl]benzotriazole to form a synergistic effect, giving the material a long-lasting ultraviolet light absorption effect. At the same time, the presence of the benzene ring in the molecule greatly enhances the steric hindrance effect, hinders the slip of the molecule, and gives the material excellent precipitation resistance, ensuring the integrity of the material.

[0026] In some embodiments of the present application, the light stabilizer is one or more of bis(2,2,6,6-tetramethylpiperidinyl)sebacate, poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinethanol) succinate and poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediol[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}.

[0027] In some embodiments, the light stabilizer includes poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinethanol) succinate and poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediol[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}. The two are used in combination to form a good synergistic effect, which reduces the amount of addition while enhancing the processing thermal stability of the material and giving the material excellent precipitation resistance and water extraction resistance.

[0028] In some embodiments of the present application, the primary antioxidant is one or more of 1,3,5-trimethyl-2,4,6-(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid (3114), 2,2'-oxalyl-bis[ethyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)]propionate, 1,3,5-tris[[4-(1,1-dimethylethyl)-3-hydroxy-2,6-dimethylphenyl]methyl]-1,3,5-triazine-2,4,6-trione and 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane.

[0029] In some embodiments of the present application, the secondary antioxidant is one or more of dilauryl thiodipropionate, dioctadecyl thiodipropionate, dilauryl thiodipropionate, tris(2,4-di-tert-butylphenyl) phosphite and dioctadecyl pentaerythritol diphosphite.

[0030] In some embodiments of the present application, the anion adsorbent is one of hydrotalcite or hydrotalcite-like material and lignocellulose anion exchanger.

[0031] The present application also provides a polyethylene material in an embodiment, comprising 93wt%-98wt% of polyethylene and 2wt%-7wt% of the composition for polyethylene material described in any one of the aforementioned embodiments.

[0032] The present application also provides an embodiment of a method for preparing the polyethylene material described in the aforementioned embodiment, wherein the mixed raw materials are put into a co-rotating twin-screw granulation device for granulation to obtain a modified polyethylene material, wherein the material temperature is 160°C-230°C.

[0033] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0034] The following embodiments specifically include the following steps:

[0035] 1. Accurately weigh the raw materials according to the formula ratio.

[0036] 2. Through the stirring equipment, the components in the formula are fully stirred to achieve full uniformity at the physical level. The stirred raw materials are put into the co-rotating twin-screw granulation equipment, and the processing temperature is controlled at 160℃-230℃ to granulate to obtain the modified material.

[0037] 3. Test the mechanical properties, antibacterial properties and anti-ultraviolet aging properties of the materials.

[0038] Example 1 and Comparative Examples 1-6

[0039] A UV-resistant and antibacterial polyethylene material is prepared, wherein the polyethylene substrate is PE-RT, and the preparation method is as follows:

[0040] (1) Accurately weigh each component according to the following formula ratio.

[0041]

[0042]

[0043] (2) Use a blender to blend the ingredients for more than 10 minutes.

[0044] (3) Use a co-rotating twin-screw granulator to granulate, and control the processing temperature at 160°C-230°C.

[0045] (4) Test the various properties of the granulated modified materials and see if they meet the requirements in the following table.

[0046]

[0047]

[0048] Stabilizers 622 and 944 are compounded to form a light stabilizer compound system with the same mechanism of action. Through the mechanisms of capturing free radicals, decomposing hydroperoxides, quenching excited state energy, etc., the two light stabilizers complement each other, the role of active groups is strengthened, and the synergistic effect is fully exerted.

[0049] The combination of UV-531 and UV-5411 is a combination system of two ultraviolet light absorbers with different action mechanisms. Compared with the use of only one ultraviolet light absorber, it can expand the wavelength range of ultraviolet light absorbed and cooperate with each other to give the material a wide range and long-lasting ultraviolet light absorption effect.

[0050] Antioxidant 1330 and antioxidant 3114, two antioxidants with the same mechanism of action, produce a synergistic effect, so that the antioxidant that is consumed first can be "regenerated" in time and resume its antioxidant effect. In the process of repeated "regeneration", the other antioxidant that is consumed can generate free radicals and still have an antioxidant effect.

[0051] Antioxidant 412s is compounded with antioxidants 1330 and 3114. 1330 and 3114 are free radical "capture bodies", and 412s is a hydroperoxide decomposer. The former is consumed first to generate ROOH, and the latter decomposes ROOH. In this process, the former is "regenerated" and plays an antioxidant role again.

[0052] The antioxidant system, UV absorber and light stabilizer form a synergistic effect. Both the light aging and thermal oxidative aging processes are free radical chain reactions. The free radicals generated during the bond aging process will consume the antioxidants. The use of light stabilizers can reduce the free radicals generated by light aging and reduce the consumption of antioxidants. The presence of antioxidants stabilizes the product and protects the light stabilizer with poor thermal stability, allowing it to fully exert its light stabilization effect, thereby improving the light, heat and oxygen stability of the product.

[0053] Light stabilizers and UV absorbers form a synergistic effect. It is impossible for UV absorbers dispersed in the resin to absorb all the UV light, but when used together with light stabilizers, the unabsorbed UV light can be released through photophysical processes, thereby avoiding damage to the polymer.

[0054] The selection of the above additives fully considers the extraction resistance, water precipitation resistance, processing thermal stability, hot and cold water usage scenarios and long-term light, heat and oxygen aging performance, fully ensuring the integrity of the material and its use in pipes for transporting hot and cold water.

[0055] The presence of LDHs adsorbent can reduce the use of antioxidants, while ensuring the removal and purification of chloride ions in water, making the overall material more cost-effective.

[0056] Silver / activated carbon and Ag / ZnO are used in combination to improve the antibacterial efficiency and long-term antibacterial properties of the material.

[0057] Embodiment 2:

[0058] A UV-resistant and antibacterial polyethylene material is prepared, wherein the polyethylene substrate is PE-RT, and the preparation method is as follows:

[0059] (1) Accurately weigh each component according to the following formula ratio.

[0060]

[0061]

[0062] (2) Use a blender to blend the ingredients for more than 10 minutes.

[0063] (3) Use a co-rotating twin-screw granulator to granulate, and control the processing temperature at 160°C-230°C.

[0064] (4) Test the various properties of the granulated modified materials and see if they meet the requirements in the following table.

[0065]

[0066] When antioxidant 1330 is fully used, its addition amount needs to be appropriately increased to ensure the long-term aging performance of the material.

[0067] LDHs adsorbent can be replaced by lignocellulosic anion adsorbent, but the added amount needs to be appropriately increased to ensure the chlorine resistance of the material.

[0068] UV-531 can be used in place of UV-5431, but the amount added needs to be appropriately increased to achieve the same UV absorption effect.

[0069] Silver / activated carbon can be replaced by Ag-Cu / SiO2, but the amount added needs to be appropriately increased to ensure the antibacterial properties of the material.

[0070] When fully using light stabilizer 944, the dosage needs to be appropriately increased to ensure the long-term light and heat stability of the material.

[0071] This example is an alternative to Example 1. The OIT value of the material is reduced, but the overall performance, extraction resistance, cost performance and safety of use can still be guaranteed.

[0072] Preparation of an anti-ultraviolet and antibacterial polyethylene material, the polyethylene substrate is PE-RT:

[0073] (1) Accurately weigh each component according to the following formula ratio.

[0074]

[0075] (2) Use a blender to blend the ingredients for more than 10 minutes.

[0076] (3) Use a co-rotating twin-screw granulator to granulate, and control the processing temperature at 160°C-230°C.

[0077] (4) Test the various properties of the granulated modified materials and see if they meet the requirements in the following table.

[0078]

[0079]

[0080] This comparative example uses 168 as an auxiliary antioxidant, and its addition amount needs to be increased, but the overall OIT value of the material is still significantly lower than that of Example 1.

[0081] The material prepared in this comparative example was compared with the material prepared in Example 1 at room temperature for three months. It was found that precipitation occurred on the particle surface of the material in this comparative example, and the precipitation resistance requirement that the material must meet was not met.

[0082] The material prepared in this comparative example was subjected to a comparative test with the material prepared in Example 1 by boiling in water at 80°C for one month. The surface precipitation of the material in this comparative example was obvious, and the material requirements were not met.

[0083] It can be concluded from this comparative example that the use of 412s as an auxiliary antioxidant can better meet the material's requirements for extraction resistance and long-term aging performance.

[0084] Comparative Example 8:

[0085] Preparation of an anti-ultraviolet and antibacterial polyethylene material, the polyethylene substrate is PE-RT:

[0086] (1) Accurately weigh each component according to the following formula ratio.

[0087]

[0088]

[0089] (2) Use a blender to blend the ingredients for more than 10 minutes.

[0090] (3) Use a co-rotating twin-screw granulator to granulate, and control the processing temperature at 160°C-230°C.

[0091] (4) Test the various properties of the granulated modified materials and see if they meet the requirements in the following table.

[0092]

[0093] This comparative example uses antioxidant 1010 as the main antioxidant. Compared with Example 2, OIT is significantly improved, indicating that antioxidant 1010 imparts excellent aging resistance to the material.

[0094] The material prepared in this comparative example was compared with the material prepared in Example 2 at room temperature for three months. There was obvious precipitation on the particle surface of the material in this comparative example, while there was no change in Example 2, and the precipitation resistance requirement that the material must meet was not met.

[0095] It can be concluded from this comparative example that the main antioxidants 1330 and 3114 can better meet the material's required extraction resistance and meet the material's safety requirements for use in hot and cold water transportation scenarios.

[0096] The present invention uses an antioxidant, a light stabilizer, an ultraviolet absorber and an anion adsorbent to perform blending modification on a PE-RT material. When selecting materials, the water extraction resistance, migration resistance, processing thermal stability and synergistic effect between the additives are taken into consideration. An additive with a large molecular structure steric effect and a large molecular weight is selected to ensure the long-term light aging performance, antibacterial performance, chlorine resistance and long-term mechanical properties of the material, and prepares an ultraviolet resistant, antibacterial and chlorine resistant polyethylene material for PE-RT pipes of water purifiers.

[0097] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A composition for polyethylene material, characterized in that: The composition comprises 0.5-5 parts by weight of an antibacterial agent, 0.1-0.5 parts by weight of anion adsorbent, 0.1-0.5 parts by weight of ultraviolet absorber, 0.1-0.5 parts by weight of light stabilizer, 0.1-0.5 parts by weight of primary antioxidant and 0.2-1 parts by weight of secondary antioxidant; The light stabilizer includes poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinylethanol) succinate and poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}; The ultraviolet absorber includes 2-hydroxy-4-n-octyloxybenzophenone and 2-[2-hydroxy-5-(1,1,3,3-tetramethylbutyl)phenyl]benzotriazole; The main antioxidants are 1,3,5-trimethyl-2,4,6-(3,5-di-tert-butyl-4-hydroxybenzyl)benzene and 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid; The secondary antioxidant is dilauryl thiodipropionate.

2. The composition for polyethylene material according to claim 1, characterized in that: The antibacterial agent is one or more of Ag-Cu / SiO2, silver / activated carbon, Ag / ZnO and chitosan.

3. The composition for polyethylene material according to claim 1, characterized in that: The anion adsorbent is one of hydrotalcite or hydrotalcite-like material and lignocellulose anion exchanger.

4. A polyethylene material, characterized in that: The method comprises 93wt%-98wt% of polyethylene and 2wt%-7wt% of the composition for polyethylene material according to any one of claims 1 to 3.

5. A method for preparing the polyethylene material according to claim 4, characterized in that: The mixed raw materials are put into a co-rotating twin-screw granulation equipment for granulation to obtain a modified polyethylene material, wherein the material temperature is 160°C-230°C.