A Zr-containing high-strength fine-grained 6-series aluminum alloy extruded bar and its manufacturing method and application

By adding Zr to the aluminum alloy to form the Al3Zr phase and refine the grains, the problems of low strength and coarse crystal layer of the traditional 6-series aluminum alloy are solved, and high-strength, high-fine crystalline aluminum alloy extruded rods are prepared, suitable for automobiles Structural materials improve the mechanical properties and stability of the materials.

CN116179877BActive Publication Date: 2024-12-03SHANDONG YANCON LIGHT ALLOY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211723368.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-12-03
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

Traditional 6-Series aluminum alloys have low strength in high-speed and harsh transportation vehicles environments. The existence of coarse crystal layer leads to a significant reduction in mechanical properties and fatigue strength, making it difficult to meet the needs of harsh environments.

Method used

Add Zr to the aluminum alloy to form the Al3Zr phase as heterogeneous nucleation, refine the grains, improve the nucleation rate, and prepare high-strength, high-fine crystalline 6-series aluminum alloy extruded rods, through specific heat treatment and mechanical processing Methods, including homogenization treatment, extrusion, solution treatment and stretching, control grain size and mechanical properties.

Benefits of technology

It significantly improves the strength and stability of aluminum alloy, reduces the depth of the coarse crystal layer, improves the comprehensive performance, is suitable for industrial production and on-site applications, has a low cost, and meets the requirements of automotive structural materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004028909200000051
    Figure BDA0004028909200000051
Patent Text Reader

Abstract

The present invention relates to the technical field of aluminum alloy profiles, and specifically to a Zr-containing high-strength fine-grained 6-series aluminum alloy extruded rod, and a manufacturing method and application thereof. The manufacturing method comprises the following steps: (1) casting; (2) homogenization treatment; (3) extrusion; (4) online solution treatment; (5) tension stretching; (6) artificial aging. The present invention adds Zr to the aluminum alloy so that fine Al3Zr phase is precipitated in the aluminum alloy, and the Al3Zr phase is used as the core of heterogeneous nucleation to increase the nucleation rate and refine the grains. The prepared aluminum alloy extruded rod has high strength, small coarse grain layer depth, stable quality, good comprehensive performance, low cost, and is suitable for industrial mass production and on-site application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy profiles, and in particular to a Zr-containing high-strength fine-grained 6-series aluminum alloy extruded bar and a manufacturing method and application thereof. Background Art

[0002] With the progress of society and the development of economy, transportation vehicles are gradually developing towards high speed, high power and light weight. 6 series aluminum alloy is an aluminum alloy with magnesium and silicon as the main alloying elements and Mg2Si phase as the strengthening phase. It is a heat-treatable aluminum alloy. 6 series aluminum alloy has the advantages of medium strength, high corrosion resistance, no tendency of stress corrosion cracking, good welding performance, unchanged corrosion performance of welding area, good formability and process performance, etc., and is widely used in the automotive parts manufacturing industry.

[0003] At present, the 6 series aluminum alloy grades mainly include 6005, 6009, 6010, 6061, 6063, 6082, 6201, 6262, 6463, 6A02, etc., among which 6005 can be used to produce ladders and antennas, 6009 and 6010 can be used to produce automobile bodies, 6061 can be used to produce pipes, bars, plates or profiles for trucks and trams, etc., 6262 can be used to produce high-stress parts with threads, 6463 can be used to produce automobile decorative parts with bright surfaces after anodizing treatment, and 6A02 can be used to produce aircraft engine parts and complex-shaped forgings and die forgings.

[0004] While 6 series aluminum alloys are widely used, some problems also arise. Traditional 6 series aluminum alloys cannot meet the more severe and harsh operating environment of transport vehicles. The presence of coarse grain layer significantly reduces the mechanical properties and fatigue strength of the material. Improving the strength of the material and controlling the coarse grain are issues that need to be urgently addressed in the industry at this stage. Summary of the invention

[0005] In view of the technical problems that traditional 6 series aluminum alloys have low strength and a coarse-grained layer, the present invention provides a high-strength and fine-grained 6 series aluminum alloy extruded rod containing Zr, and a manufacturing method and application thereof. The present invention adds Zr to the aluminum alloy to precipitate fine Al3Zr phase in the aluminum alloy, and uses the Al3Zr phase as the core of heterogeneous nucleation to increase the nucleation rate and refine the grains. The prepared aluminum alloy extruded rod has high strength, a small coarse-grained layer depth, stable quality, good comprehensive performance, and low cost, and is suitable for industrial mass production and on-site application.

[0006] In a first aspect, the present invention provides a method for manufacturing a Zr-containing high-strength fine-grained 6-series aluminum alloy extruded bar, comprising the following steps: (1) preparing a Zr-containing high-strength fine-grained 6-series aluminum alloy extruded bar according to Si 0.8wt% to 1.3wt%, Fe≤0.35wt%, Cu 0.4wt% to 0.6wt%, Mn 0.4wt% to 0.7wt%, Mg0.8wt% to 1.2wt%, Cr 0.1wt% to 0.3wt%, Ti≤0.06wt%, and Zr (1) preparing the raw materials by mixing the raw materials with the proportion of 0.1wt% to 0.2wt%, Pb≤0.01wt%, single impurity≤0.05wt%, total impurity≤0.15wt%, and the balance Al, smelting, and then casting into round cast rods; (2) homogenizing the round cast rods, heating the round cast rods to 510-540°C, keeping them warm for 8-10 hours, and then cooling the round cast rods, air cooling for 30-60 minutes, and water cooling for 30-50 minutes; (3) extruding to obtain rods with a diameter of 50-100 mm; (4) directly cooling the rods online with water for solid solution treatment, and controlling the temperature of the rods after exiting the water to be less than 80°C; (5) stretching the water-cooled rods; (6) keeping the rods at 160-180°C for 8-10 hours for artificial aging.

[0007] Furthermore, in step (1), after the charge is deposited, a sodium-free covering agent is evenly sprinkled on it to fully cover it, and it is smelted at a temperature of 710-750°C for 200-400 minutes, during which electromagnetic stirring is performed. After the charge is completely melted, the slag is removed and the sodium-free covering agent is evenly sprinkled on it, and the slag is removed again after 3-5 minutes.

[0008] Furthermore, the heating rate of step (2) is 10-15°C / min.

[0009] Furthermore, before extrusion in step (3), the round cast rods are first subjected to 100% ultrasonic flaw detection, and round cast rods whose ultrasonic flaw detection grade meets the A-level requirement in GB / T 6519 are selected, and the round cast rods are lathe-cut.

[0010] Furthermore, the extrusion parameters of step (3) are as follows: mold temperature is 430-500°C, round cast rod temperature is 490-520°C, extrusion speed is 2-4 mm / s, and outlet temperature is >525°C.

[0011] Furthermore, the stretching deformation in step (5) is 0.5% to 1.5%.

[0012] In a second aspect, the present invention provides a Zr-containing high-strength and fine-grained 6-series aluminum alloy extruded bar prepared by the above-mentioned manufacturing method.

[0013] In a third aspect, the present invention also provides a use of the above-mentioned Zr-containing high-strength fine-grained 6-series aluminum alloy extruded rod as an automobile structural material.

[0014] The beneficial effects of the present invention are:

[0015] The present invention defines the composition of the aluminum alloy of the rod, wherein Si is defined as 0.8wt% to 1.3wt%, M is defined as 0.8wt% to 1.2wt%, and the mass ratio of Mg to Si is less than the normal mass ratio of 1.73 when Mg and Si completely generate the strengthening phase Mg2Si, that is, the Si element of the present invention is slightly excessive, the purpose is to eliminate the adverse effects of impurity elements such as Fe on the performance of the aluminum alloy; Fe≤0.30wt% to prevent the alloy grain structure from being coarse and avoid the generation of needle-shaped FeAl3, thereby adversely affecting the mechanical properties of the alloy; Cu is defined as 0 .4wt%~0.6wt%, improve the strength and hardness of the alloy, promote the uniform nucleation of Mg and Si precipitation phases, accelerate the aging strengthening process of the alloy, increase the heat treatment strengthening effect, and reduce the negative impact of Cu on the corrosion resistance of the alloy; add Cr to refine the grains, make the grains after recrystallization slender, improve the corrosion resistance of the alloy, and improve the strength after artificial aging; limit Mn to 0.4wt%~0.7wt%, the purpose is to form fine and dispersed second phase particles in the alloy to hinder the recrystallization of the alloy, refine the grains, and improve the alloy The mechanical properties of the alloy are improved, and the AlMnSi phase is avoided due to excessive Mn content and the strengthening phase Mg2Si, which causes the alloy strengthening effect to decrease; trace Ti elements are added to refine the grains, so that the alloy obtains higher strength and elongation after refinement. In the subsequent heat treatment process, Ti can be melted into the α-Al solid solution, and precipitation strengthening occurs during artificial aging, thereby improving the strength of the alloy; Zr is limited to 0.1wt% to 0.2wt%, and the Al3Zr dispersed phase particles formed by Zr and Al can serve as the heterogeneous nucleation core of α-Al during the alloy solidification process, playing a good role in transformation. The quality effect greatly refines the grains, improves the cast structure of the alloy, and improves the mechanical properties of the alloy. In addition, during the heat treatment process, a secondary fine Al3Zr dispersed phase will be formed in the alloy, which is evenly dispersed in the grain boundaries and dislocations of the aluminum matrix, playing a dispersion strengthening and pinning role, inhibiting recrystallization and hindering the merging and growth of grains, thereby reducing the depth of the coarse-grained layer. With the increase of Zr addition, the grain size gradually decreases, the mechanical properties of the alloy gradually increase, and the grain size gradually decreases. When Zr>0.2wt%, coarse dendrites appear in the alloy and the mechanical properties decrease.

[0016] Secondly, the manufacturing method provided by the present invention has high production efficiency, short production cycle, low production cost, and the manufactured aluminum alloy extruded bar has good tensile properties (R m ≥410MPa, R p0.2 ≥396MPa, A 50 ≥12%), the depth of low-magnification coarse-grained layer is small (≤1.0mm), and it has obvious economic benefits. DETAILED DESCRIPTION

[0017] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0018] Example 1

[0019] A rod with a diameter of 58 mm has the following composition:

[0020] Si: 0.88wt%, Fe: 0.14wt%, Cu: 0.58wt%, Mn: 0.45wt%, Mg: 0.83wt%, Cr: 0.12wt%, Ti: 0.04wt%, Zr: 0.16wt%, Pb: 0.002wt%, the balance is Al and unavoidable impurities, a single impurity ≤ 0.05wt%, a total impurity ≤ 0.15wt%;

[0021] It is prepared by the following manufacturing method:

[0022] (1) Casting: Mix the ingredients according to the proportion, melt at 730-750℃, and then cast into round cast bars;

[0023] Electromagnetic stirring is performed during the smelting process. After the charge is deposited, sodium-free covering agent is evenly sprinkled to fully cover it. After all the charge is melted, the slag is removed and sodium-free covering agent is evenly sprinkled. The slag is removed again after 5 minutes.

[0024] (2) Homogenization treatment: The round cast rod was heated to 540°C at a heating rate of 10°C / min and kept at this temperature for 8 hours. The cast rod was then air-cooled for 45 minutes and water-cooled for 40 minutes to obtain a round cast rod that had undergone homogenization treatment.

[0025] 100% ultrasonic flaw detection is performed on round cast bars, and round cast bars with ultrasonic flaw detection grade meeting the requirements of Grade A in GB / T 6519 are selected, and the round cast bars are rolled to a diameter of 248mm;

[0026] (3) Extrusion treatment: The mold is heated to 430°C and kept warm for 8 hours, and the round cast rod is heated to 520°C for extrusion. The extrusion speed is 2.5 mm / s, and the outlet temperature is >525°C to obtain a rod with a diameter of 58 mm.

[0027] (4) Online solution treatment: The rod is directly water-cooled online to control the temperature of the rod after exiting the water to less than 80°C;

[0028] (5) Tension stretching: The water-cooled bar is stretched to a deformation of 1.2%;

[0029] (7) Artificial aging: The bar is kept at 170°C for 8 h for single-stage artificial aging treatment.

[0030] The aluminum alloy bar obtained in Example 1 was subjected to mechanical property tests, and the test results are as follows:

[0031] Tensile properties: R m 440MPa, R p0.2 is 422MPa, A 50 15%;

[0032] The depth of the coarse grain ring is ≤1mm.

[0033] The mechanical properties of this aluminum alloy bar are higher than the requirements of GB / T 3191-2019 aluminum and aluminum alloy extruded bars; at the same time, the coarse grain ring depth is ≤1mm, the performance is stable, and it can be used as an automotive structural material, effectively ensuring the safety and reliability of the vehicle.

[0034] At the same time, the ingredients were changed and the aluminum alloy bars (Comparative Examples 1 to 3) were manufactured according to the manufacturing method of Example 1. The tensile properties and coarse grain ring depths of the aluminum alloy bars of Example 1 and Comparative Examples 1 to 3 were compared.

[0035] Table 1 Composition of Example 1 and Comparative Examples 1 to 3 (balance is aluminum and impurities, unit: wt%)

[0036] project Si Fe Cu Mn Mg Cr Ti Zr Pb Example 1 0.88 0.14 0.58 0.45 0.83 0.12 0.04 0.16 0.002 Comparative Example 1 0.89 0.13 0.58 0.42 0.85 0.11 0.04 0 0.002 Comparative Example 2 0.91 0.15 0.56 0.41 0.85 0.12 0.04 0.04 0.002 Comparative Example 3 0.86 0.15 0.54 0.43 0.84 0.11 0.05 0.23 0.002

[0037] Table 2 Tensile properties and coarse grain ring depth of Example 1 and Comparative Examples 1 to 3

[0038]

[0039] Example 2

[0040] A rod with a diameter of 90 mm has the following composition:

[0041] Si: 0.86wt%, Fe: 0.15wt%, Cu: 0.54wt%, Mn: 0.45wt%, Mg: 0.83wt%, Cr: 0.11wt%, Ti: 0.04wt%, Zr: 0.18wt%, Pb: 0.002wt%, the balance is Al and unavoidable impurities, a single impurity ≤ 0.05wt%, a total impurity ≤ 0.15wt%;

[0042] The manufacturing method of the aluminum alloy profile comprises the following steps:

[0043] (1) Casting: Melting according to the proportion of ingredients, melting at 730-750℃, and then casting into round cast bars;

[0044] Electromagnetic stirring is performed during the smelting process. After the charge is deposited, sodium-free covering agent is evenly sprinkled to fully cover it. After all the charge is melted, the slag is removed and sodium-free covering agent is evenly sprinkled. The slag is removed again after 3 minutes.

[0045] (2) Homogenization treatment: The round cast rod was heated to 510°C at a heating rate of 15°C / min and kept at this temperature for 10 hours. The cast rod was then air-cooled for 60 minutes and water-cooled for 30 minutes to obtain a round cast rod that had undergone homogenization treatment.

[0046] 100% ultrasonic flaw detection is performed on round cast bars. Round cast bars with ultrasonic flaw detection grade meeting the requirements of Grade A in GB / T 6519 are selected, and the round cast bars are rolled to a diameter of 308mm.

[0047] (3) Extrusion treatment: The mold is heated to 470°C and kept warm for 10 hours, and the round cast rod is heated to 490°C for extrusion. The extrusion speed is 3.8 mm / s, and the outlet temperature is >525°C to obtain a rod with a diameter of 90 mm.

[0048] (4) Online solution treatment: After extrusion, online water cooling is carried out directly to control the temperature of the bar after exiting the water to less than 80°C;

[0049] (5) Tension stretching: The water-cooled bar is stretched to a deformation of 1.5%;

[0050] (6) Artificial aging: The bar is kept at 175°C for 8 h for single-stage artificial aging treatment.

[0051] The aluminum alloy bar obtained in Example 2 was subjected to mechanical property tests, and the test results are as follows:

[0052] Tensile properties: R m 428MPa, R p0.2 403MPa, A 50 15.5%;

[0053] The depth of the coarse grain ring is ≤1mm.

[0054] The mechanical properties of this aluminum alloy bar are higher than the requirements of GB / T 3191-2019 aluminum and aluminum alloy extruded bars; at the same time, the coarse grain ring depth is ≤1mm, the performance is stable, and it can be used as an automotive structural material, effectively ensuring the safety and reliability of the vehicle.

[0055] Although the present invention has been described in detail by way of preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and such modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily conceive of changes or substitutions within the technical scope disclosed by the present invention, and such changes or substitutions shall be within the scope of protection of the present invention.

Claims

1. A method for manufacturing a Zr-containing high-strength fine-grained 6-series aluminum alloy extruded bar, It is characterized in that The method comprises the following steps: (1) preparing materials according to the proportion of Si 0.8wt%~1.3wt%, Fe≤0.35wt%, Cu 0.4wt%~0.6wt%, Mn 0.4wt%~0.7wt%, Mg 0.8wt%~1.2wt%, Cr 0.1wt%~0.3wt%, Ti≤0.06wt%, Zr 0.1wt%~0.2wt%, Pb≤0.01wt%, individual impurities≤0.05wt%, total impurities≤0.15wt%, and the balance Al, smelting, and then casting into round cast rods; (2) homogenizing the round cast rods, heating the round cast rods to 510~540°C, keeping the temperature for 8~10h, and then cooling the round cast rods, air cooling for 30~60min, and water cooling for 30~50min; (3) extruding The obtained rods have a diameter of 50-100 mm, and the extrusion parameters are as follows: the die temperature is 430-500°C, the round cast rod temperature is 490-520°C, the extrusion speed is 2-4 mm / s, and the outlet temperature is >525°C; (4) the rods are directly water-cooled online for solution treatment, and the temperature of the rods after exiting the water is controlled to be <80°C; (5) the water-cooled rods are stretched; (6) the rods are kept at 160-180°C for 8-10 h for artificial aging.

2. The manufacturing method according to claim 1, It is characterized in that In step (1), after the charge is deposited, a sodium-free covering agent is evenly sprinkled on it to fully cover it. The charge is smelted at a temperature of 710-750°C for 200-400 min, during which electromagnetic stirring is performed. After the charge is completely melted, the slag is removed and the sodium-free covering agent is evenly sprinkled on it. The slag is removed again after 3-5 min.

3. The manufacturing method according to claim 1, It is characterized in that The heating rate of step (2) is 10-15°C / min.

4. The manufacturing method according to claim 1, It is characterized in that Before extrusion in step (3), 100% ultrasonic flaw detection is performed on the round cast bars, and round cast bars whose ultrasonic flaw detection level meets the A-level requirement in GB / T 6519 are selected, and the round cast bars are lathe-cut.

5. The manufacturing method according to claim 1, It is characterized in that The tensile deformation in step (5) is 0.5% to 1.5%.

6. A Zr-containing high-strength fine-grained 6-series aluminum alloy extruded bar prepared by the manufacturing method as described in any one of claims 1 to 5.

7. Use of the Zr-containing high-strength fine-grained 6-series aluminum alloy extruded bar as claimed in claim 6 as an automobile structural material.

Citation Information

Patent Citations

  • High-strength Al-Mg-Si-Mn deforming aluminum alloy and preparing method thereof

    CN109666824A