A controllable modification method for improving the hydrophilicity of hollow fiber membranes
Through in-situ modification and step-by-step synthesis methods, the problem of poor graft uniformity in the prior art is solved, the pore size distribution uniformity and pollution resistance of the membrane are improved, and the use is extended life.
Patent Information
- Application Number
- CN202310421419.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-04-19
Smart Images

Figure CN116196781B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of separation membranes, and in particular relates to a controllable modification method for improving the hydrophilicity of a hollow fiber membrane. Background Art
[0002] Membrane separation technology is a highly efficient separation process that combines concentration, purification, and refinement. It is widely used in water treatment, material separation, food, chemical industry, biomedicine, and other fields due to its advantages of low energy consumption, high efficiency, no phase change, and mild operating conditions. Among them, hollow fiber membrane is one of the main forms of separation membranes. The pore size of hollow fiber membranes is generally between 10nm-100μm, which can be used to intercept colloids, particles, proteins and other macromolecules in water.
[0003] The material of hollow fiber membrane mainly includes polyethylene, polypropylene, poly-4-methyl-1-pentene, polyvinylidene fluoride, polytetrafluoroethylene, polysulfone, polyethersulfone etc. at present, and the membrane of these materials usually has strong hydrophobicity, so that the membrane is easy to adsorb protein, resulting in a decrease in water flux, a decrease in service life, etc. In order to improve the hydrophilicity of the membrane, a hydrophilic functional group can be introduced in the membrane surface or pores using a bulk modification method. The bulk modification method is usually to add a hydrophilic modifier to the casting solution, that is, to achieve the modification of the membrane by physical blending during film formation, with the advantages of simple operation and low cost, but the method of this physical blending can cause the membrane structure to change, and the stability and dispersibility of the modifier are poor, thereby affecting the anti-pollution ability of the membrane, resulting in a sharp attenuation of the water flux of the membrane.
[0004] At present, most of the surface grafting methods are used to introduce hydrophilic functional groups on the membrane surface or in the pores to avoid the membrane performance degradation caused by the defects of physical blending. For example, patent document CN102516584A discloses a modification method for polyvinylidene fluoride microporous membrane anti-protein contamination, and the surface grafting modification of polyvinylidene fluoride membrane is realized by free radical polymerization and initiated polymerization; Patent document CN109174062A discloses a heavy metal ion adsorption type PVDF modified separation membrane, and PAMAM dendritic polymer is directly grafted on the PVDF separation membrane. However, the grafting uniformity of the above method is poor, resulting in uneven pore size distribution of the membrane (pore size distribution includes size distribution and position distribution of the pores), which is not conducive to the improvement of membrane performance. Therefore, how to overcome the defects of poor grafting uniformity in the above method, so as to improve the pore size distribution uniformity of the hollow fiber membrane, and further improve the pollution resistance and flux attenuation rate, is a technical problem to be solved in this field. Summary of the invention
[0005] The controllable modification method for improving the hydrophilicity of the hollow fiber membrane provided by the present invention adopts the method of in-situ modification and step-by-step synthesis, which can achieve uniform grafting of modified molecules on the hollow fiber membrane, maximize the uniformity of the pore size distribution of the membrane, and further improve the pollution resistance and flux attenuation rate of the modified hollow fiber membrane.
[0006] A first aspect of the present invention provides a controllable modification method for improving the hydrophilicity of a hollow fiber membrane, comprising the following steps:
[0007] (1) placing an aminated hollow fiber membrane raw material in a solution containing an olefin monomer, reacting at 10-70° C. for 1-24 hours to obtain a fiber membrane intermediate;
[0008] The fiber membrane intermediate is placed in a solution containing a polyamine monomer, and reacted at 10-70° C. for 1-24 hours to obtain a primary modified hollow fiber membrane;
[0009] (2) Using the once modified hollow fiber membrane as a raw material, repeat step (1) once to obtain a modified hollow fiber membrane.
[0010] The modification method as described above, wherein the modified hollow fiber membrane is further subjected to cross-linking treatment;
[0011] The cross-linking treatment comprises: placing the modified hollow fiber membrane in a solution containing a cross-linking agent for reaction at 20-70°C.
[0012] The modification method as described above, wherein after step (2), it further comprises: repeating step (1) N times on the modified hollow fiber, 1≤N≤19.
[0013] In the modification method as described above, the olefinic monomer includes at least one of methyl acrylate, ethyl acrylate, propyl acrylate, acrylamide, N-ethylacrylamide, N,N'-methylenebisacrylamide, and N-propylacrylamide.
[0014] In the modification method as described above, the polyamine monomer includes at least one of ethylenediamine, propylenediamine, 1,2,3-propylenetriamine, diethylenetriamine, and N-aminoethylpiperazine.
[0015] The modification method as described above, wherein the mass ratio of the ethylenic monomer to the polyamine monomer is (1:3) to (3:1).
[0016] In the modification method as described above, the cross-linking agent includes at least one of maleic anhydride, trimesic acid, malonic acid, succinic acid, malic acid, citric acid, polyacrylic acid, polymethacrylic acid, polystyrene sulfonic acid, and polyvinyl sulfonic acid.
[0017] The modification method as described above, wherein the concentration of the olefinic monomer in the solution containing the olefinic monomer is 0.1-30wt%, and the volume ratio of the solution containing the olefinic monomer to the aminated hollow fiber membrane raw material is (2:1)-(100:1);
[0018] In the modification method as described above, the concentration of the polyamine monomer in the solution containing the polyamine monomer is 0.1-30 wt %, and the volume ratio of the solution containing the polyamine monomer to the aminated hollow fiber membrane raw material is (2:1)-(100:1).
[0019] The modification method as described above, wherein the grafting rate of the modified hollow fiber membrane is 3-20%.
[0020] The implementation of the present invention has at least the following beneficial effects:
[0021] The modification method of the modified hollow fiber membrane provided by the present invention adopts the method of in-situ modification and stepwise synthesis, so that the olefin monomer and the polyamine monomer alternately circulate into the surface and pores of the hollow fiber membrane for reaction, and can realize uniform grafting of the modified molecules on the hollow fiber membrane, and maximize the uniform pore size distribution of the membrane, thereby further improving the pollution resistance and flux attenuation rate of the modified hollow fiber membrane. And the modified hollow fiber membrane obtained by the modification method provided by the present invention has uniform pore size distribution, can realize long-term service, and has the advantages of strong pollution resistance and low flux attenuation rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is a SEM image of the modified hollow fiber membrane in Example 1;
[0023] Figure 2 is a SEM image of the modified hollow fiber membrane in Comparative Example 1;
[0024] Figure 3 is the SEM image of the original polysulfone hollow fiber membrane;
[0025] Figure 4 It is a pore size distribution curve diagram of the original polysulfone hollow fiber membrane and Example 1, Example 3, and Comparative Example 5. DETAILED DESCRIPTION
[0026] The specific implementations listed below are only for describing the principles and features of the present invention. The examples are only used to explain the present invention and are not intended to limit the scope of the present invention. Based on the embodiments of the present invention, all other implementations obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] A first aspect of the present invention provides a controllable modification method for improving the hydrophilicity of a hollow fiber membrane, comprising the following steps:
[0028] (1) placing an aminated hollow fiber membrane raw material in a solution containing an olefin monomer, reacting at 10-70° C. for 1-24 hours to obtain a fiber membrane intermediate;
[0029] The fiber membrane intermediate is placed in a solution containing a polyamine monomer, and reacted at 10-70° C. for 1-24 hours to obtain a primary modified hollow fiber membrane;
[0030] (2) Using the once modified hollow fiber membrane as a raw material, repeat step (1) once to obtain a modified hollow fiber membrane.
[0031] In the present invention, the aminated hollow fiber membrane raw material refers to a hollow fiber membrane raw material having amino groups on the surface, which can be obtained by conventional methods. For example, the hollow fiber membrane raw material is first immersed in a solution containing a nitro compound to perform a nitration treatment, and then immersed in a solution containing an amino compound to complete the amination treatment, so that the surface and pores of the hollow fiber membrane raw material have amino groups, thereby obtaining an aminated hollow fiber membrane raw material.
[0032] In step (1), the amino groups on the aminated hollow fiber membrane raw material are used as the core reaction sites, and the olefin monomers and polyamine monomers are sequentially introduced into the surface and pores of the hollow fiber membrane raw material to react, thereby obtaining a first-modified hollow fiber membrane. In this way, the present invention adopts an in-situ modification method, and each time the olefin monomers and polyamine monomers react once, a modified layer (also called "generation") is added to the hollow fiber membrane raw material. By analogy, the present invention also adopts a stepwise synthesis method, and uses the first-modified hollow fiber membrane as a raw material, repeats step (1) once, and adds two modified layers to the hollow fiber membrane raw material to obtain a second-modified hollow fiber membrane, which can be directly used as a modified hollow fiber membrane.
[0033] The modified layer is composed of modified molecules with a dendritic structure. Each modified layer at least includes a connecting unit and an extending unit, each connecting unit connects two extending units, and the nitrogen atom on the connecting unit is connected to the carbon atom of the amide bond in the extending unit.
[0034] According to the technical solution of the present invention, the above-mentioned modification method can be used to prepare a modified hollow fiber membrane with strong pollution resistance and low flux attenuation rate. Based on this phenomenon, the inventor analyzed and believed that it might be: using the amino group on the aminated hollow fiber membrane raw material as the core reaction site, the olefin monomer and the polyamine monomer are alternately cyclically contacted with the hollow fiber membrane raw material to react, which can realize the in-situ modification of the hollow fiber membrane and the gradual synthesis of the modified layer, avoiding the phenomenon that some sites have large steric hindrance during one-time polymerization grafting, resulting in uneven grafting, while retaining the dendritic structure of the modified molecule, the modified molecule can be uniformly grafted on the hollow fiber membrane raw material, maximizing the uniformity of the pore size distribution of the membrane, thereby effectively improving the pollution resistance and flux attenuation rate of the hollow fiber membrane.
[0035] In addition, during the stepwise reaction process, the monomer concentration can be limited and the reaction time can be sufficient so that the monomers can be grafted onto the membrane surface more evenly. Through the stepwise reaction, the ungrafted sites can also have sufficient opportunities for grafting.
[0036] The surface of the modified hollow fiber membrane has a large number of amino groups, and can be directly used as a modified hollow fiber membrane, or the modified hollow fiber membrane can be cross-linked. In one embodiment, the modified hollow fiber membrane is cross-linked, and the cross-linking treatment includes: placing the modified hollow fiber membrane in a solution containing a cross-linking agent at 20-70°C for reaction. The reaction time is greater than 0 and not greater than 24h. After the cross-linking treatment, the functional groups of the modified layer can be adjusted while improving the stability of the modified layer, thereby achieving the regulation of the membrane performance.
[0037] In the present invention, after step (2), the following step is further included: repeating step (1) on the modified hollow fiber N times, 1≤N≤19. In this way, by controlling the number of repeated executions to N times, (N+1) modified layers are added to the hollow fiber membrane, so that the modified hollow fiber membrane of the present invention also has the advantage of controllable related performances. The reason is that when preparing the modified hollow fiber membrane, the olefin monomer and the polyamine monomer are alternately circulated into the surface and pores of the hollow fiber membrane for reaction, and the number of modified layers can be adjusted by controlling parameters such as the number of repeated executions, thereby achieving precise control of the grafting rate and the number of functional groups of the modified layer on the hollow fiber membrane, thereby achieving control of the average pore size of the membrane, and thus achieving high optimization of the performance of the membrane.
[0038] Therefore, the preparation method of the above-mentioned modified hollow fiber membrane can accurately control the grafting rate and the number of functional groups of the modified layer, and ultimately ensure that the modified hollow fiber membrane has a target grafting rate or a target number of functional groups, thereby ensuring that the modified hollow fiber membrane has a target average pore size. This controllability can not only achieve consistency in products of the same batch and improve production efficiency, but also facilitate the construction of differentiation of the grafting of the modified layer on the hollow fiber membrane, thereby achieving product diversity and meeting the different requirements of different environments for different pore sizes, pollution resistance and flux attenuation rates.
[0039] The present invention does not impose too many restrictions on the number of repeated executions, and the number of repeated executions can be adjusted according to actual conditions. Exemplarily, the number of repeated executions is N, 1≤N≤19. When the number of repeated executions is less than 1, it will directly lead to a small grafting rate, and it will not be possible to achieve complete modification of the membrane surface and the inside of the pores, resulting in poor hydrophilicity of the membrane surface, easy adsorption of proteins and irreversible pollution; when the number of alternating cycles is greater than 19, it will directly lead to an excessively large grafting rate, and the membrane surface and pores are prone to form a dense and thick hydrophilic layer, which in turn increases the mass transfer resistance of water and materials, resulting in a decrease in the separation efficiency of the membrane.
[0040] The present invention does not impose too many restrictions on the solution containing the olefinic monomer, which can be prepared by mixing the conventional olefinic monomer and solvent in the art. The olefinic monomer includes at least one of methyl acrylate, ethyl acrylate, propyl acrylate, acrylamide, N-ethylacrylamide, N,N'-methylenebisacrylamide, and N-propylacrylamide; the polyamine monomer includes at least one of ethylenediamine, propylenediamine, 1,2,3-propylenetriamine, diethylenetriamine, and N-aminoethylpiperazine.
[0041] The present invention does not impose too many restrictions on the solution containing the polyamine monomer, and it can be prepared by mixing conventional polyamine monomers in the art with solvents. The polyamine monomer includes at least one of ethylenediamine, propylenediamine, 1,2,3-propylenetriamine, diethylenetriamine, and N-aminoethylpiperazine.
[0042] The present invention does not impose too many restrictions on the amount of alkenyl monomer and polyamine monomer added in the above-mentioned preparation process, as long as the reaction sites on the surface of the hollow fiber membrane can fully participate in the reaction. Exemplarily, the mass ratio of alkenyl monomer to polyamine monomer is (1:3)-(3:1). Among them, alkenyl monomer refers to the mass of alkenyl monomer in a solution containing alkenyl monomer, and the mass of polyamine monomer refers to the mass of polyamine monomer in a solution containing polyamine monomer.
[0043] The present invention does not limit the specific type of cross-linking agent. The solution containing the cross-linking agent can be obtained by mixing the cross-linking agent and a solvent, wherein the cross-linking agent can be selected from organic polyacids, anionic polymers, anionic polymer salts, etc., and specifically includes at least one of maleic anhydride, trimesic acid, malonic acid, succinic acid, malic acid, citric acid, polyacrylic acid, polymethacrylic acid, polystyrene sulfonic acid, polyethylene sulfonic acid, polyacrylic acid salt, polymethacrylate, polystyrene sulfonate, and polyethylene sulfonate. The solvent includes at least one of water, methanol, ethanol, and isopropanol. The concentration of the cross-linking agent in the solution containing the cross-linking agent is 0.01-10wt%.
[0044] The present invention does not impose too many restrictions on the concentration of the monomer in the solution, as long as the addition amount is met. Exemplarily, the concentration of the olefinic monomer in the solution containing the olefinic monomer is 0.1-30wt%, and the volume ratio of the solution containing the olefinic monomer to the aminated hollow fiber membrane raw material is (2:1)-(100:1). The concentration of the polyamine monomer in the solution containing the polyamine monomer is 0.1-30wt%, and the volume ratio of the solution containing the polyamine monomer to the aminated hollow fiber membrane raw material is (2:1)-(100:1).
[0045] The solvent for preparing the monomer solution is a solvent that does not dissolve the material of the hollow fiber membrane but can dissolve the olefin monomer and the polyamine monomer used, such as at least one of water, methanol, ethanol, and isopropanol.
[0046] The present invention does not limit the main material and performance parameters of the hollow fiber membrane raw material. For example, the material of the hollow fiber membrane raw material can be at least one of polyethylene, polypropylene, poly-4-methyl-1-pentene, polyvinylidene fluoride, polytetrafluoroethylene, polysulfone, and polyethersulfone. The pore size of the hollow fiber membrane raw material can be 10nm-200μm.
[0047] The second aspect of the present invention provides a modified hollow fiber membrane obtained by the modification method provided by the first aspect.
[0048] Due to the particularity of the aforementioned preparation method, the modified layer on the modified hollow fiber membrane obtained by this method is grafted evenly, so that the pore size distribution of the membrane is uniform, has excellent pollution resistance, can achieve long-term service, and has a low flux attenuation rate, which broadens the application range of the modified hollow fiber membrane.
[0049] Specifically, the modified hollow fiber membrane of the present invention has a pure water flux that is reduced by no more than 30% compared with the original membrane, and a contact angle of less than 60°, a flux attenuation rate of less than 15% in a protein continuous filtration experiment within 2 hours, and a flux cleaning recovery rate of more than 95%. The grafting rate of the modified layer on the hollow fiber membrane is 3-20%, such as 3%, 5%, 8%, 10%, 15%, 20% or a range consisting of any two of them.
[0050] The present invention does not limit the application field of the modified hollow fiber membrane, and can be a material separation process in the biomedical field, or a sterilization and turbidity removal process in the water treatment field. Specifically, it can be applied to the separation of viruses and proteins, the separation of proteins and cells, the separation of proteins and water, etc.
[0051] The present invention will be further described below by means of specific examples and comparative examples.
[0052] Example 1
[0053] Pretreatment: In this embodiment, a polysulfone hollow fiber membrane with an average pore size of 50 nm is immersed in an isopropanol solution of 8 wt% ammonium nitrate and 73.5 wt% trifluoroacetic anhydride, and reacted at a constant temperature of 25°C for 4 hours to complete the nitration of the polysulfone hollow fiber membrane; then immersed in an isopropanol solution of tetrabutylammonium chloride at a constant temperature of 70°C for 12 hours to complete the amino modification, and washed with methanol for multiple times to obtain an amino hollow fiber membrane raw material;
[0054] (1) placing an amino polysulfone hollow fiber membrane raw material in a 3-fold volume of a 10 wt% methanol solution of methyl acrylate, reacting at 30° C. in the dark for 12 h, taking out the polysulfone hollow fiber membrane, and washing the unreacted methyl acrylate monomer in the membrane with methanol to obtain a fiber membrane intermediate;
[0055] The fiber membrane intermediate is placed in a 10 wt% methanol solution of ethylenediamine, and reacted at 30°C in the dark for 12 hours, then the fiber membrane intermediate is taken out, and the unreacted monomer is washed with methanol to obtain a primary modified hollow fiber membrane;
[0056] (2) using the once-modified hollow fiber membrane as a raw material, repeating step (1) for the fifth time to obtain a six-times-modified hollow fiber membrane;
[0057] (3) The six-times modified hollow fiber membrane was immersed in a 2 wt % polyacrylic acid aqueous solution, and the cross-linking reaction was completed at a constant temperature of 40° C. within 10 hours. After being rinsed with deionized water, a six-times modified hollow fiber membrane was obtained.
[0058] Example 2
[0059] The preparation method is basically the same as that of Example 1, except that the hollow fiber membrane modified six times in step (2) after repeating step (1) for the fifth time is replaced by a hollow fiber membrane modified four times in step (1) for three times; the hollow fiber membrane modified six times in step (3) is replaced by a hollow fiber membrane modified four times in this example, and other conditions remain unchanged.
[0060] Example 3
[0061] The preparation method is basically the same as that of Example 1, except that the hollow fiber membrane modified six times in step (2) after repeating step (1) for the fifth time is replaced by a hollow fiber membrane modified ten times after repeating step (1) for nine times; the hollow fiber membrane modified six times in step (3) is replaced by a hollow fiber membrane modified ten times in this example, and other conditions remain unchanged.
[0062] Example 4
[0063] The preparation method is basically the same as that of Example 1, except that the 2 wt % polyacrylic acid aqueous solution in step (3) of Example 1 is replaced by a 1 wt % polyacrylic acid aqueous solution, and other conditions remain unchanged.
[0064] Example 5
[0065] The preparation method is basically the same as that of Example 1, except that the 2 wt % polyacrylic acid aqueous solution in step (3) of Example 1 is replaced by a 5 wt % polyacrylic acid aqueous solution, and other conditions remain unchanged.
[0066] Example 6
[0067] The preparation method is basically the same as that of Example 1, except that the 2 wt % polyacrylic acid aqueous solution in step (3) of Example 1 is replaced by a 3 wt % citric acid aqueous solution, and other conditions remain unchanged.
[0068] Example 7
[0069] The preparation method is basically the same as that of Example 1, except that step (3) is omitted, and the six-times-modified hollow fiber membrane is directly used as the modified hollow fiber membrane, and other conditions remain unchanged.
[0070] Example 8
[0071] The preparation method is basically the same as that of Example 1, except that the methanol solution of methyl acrylate in step (1) of Example 1 is replaced by an aqueous solution of N,N'-methylenebisacrylamide, and the methanol solution of ethylenediamine is replaced by an aqueous solution of N-aminoethylpiperazine, and other conditions remain unchanged.
[0072] Example 9
[0073] The preparation method is basically the same as that of Example 1, except that the methanol solution of methyl acrylate in step (1) of Example 1 is replaced by an aqueous solution of N,N'-methylenebisacrylamide, and the methanol solution of ethylenediamine is replaced by an aqueous solution of N-aminoethylpiperazine; the hollow fiber membrane modified six times by repeating step (1) for the fifth time in step (2) is replaced by a hollow fiber membrane modified ten times by repeating step (1) for nine times; the hollow fiber membrane modified six times in step (3) is replaced by a hollow fiber membrane modified ten times in this example, and other conditions remain unchanged.
[0074] Example 10
[0075] The preparation method is basically the same as that of Example 1, except that the 50 nm polysulfone hollow fiber ultrafiltration membrane in the pretreatment of Example 1 is replaced by a 30 nm polyethersulfone hollow fiber membrane, and other conditions remain unchanged.
[0076] Embodiment 11
[0077] The preparation method is basically the same as that of Example 1, except that the six-times modified hollow fiber membrane obtained by repeating step (1) for the fifth time in step (2) is replaced by a two-times modified hollow fiber membrane obtained by repeating step (1) once; the six-times modified hollow fiber membrane in step (3) is replaced by the two-times modified hollow fiber membrane of this example, and other conditions remain unchanged.
[0078] Example 12
[0079] The preparation method is basically the same as that of Example 1, except that in step (2), "after repeating step (1) for the fifth time, a hollow fiber membrane modified six times is obtained" is replaced by "after repeating step (1) for 19 times, a hollow fiber membrane modified twenty times is obtained"; in step (3), the hollow fiber membrane modified six times is replaced by the hollow fiber membrane modified twenty times in this example, and other conditions remain unchanged.
[0080] Embodiment 13
[0081] The preparation method is basically the same as that in Example 1, except that in step (2), "after repeating step (1) for the fifth time, a hollow fiber membrane modified six times is obtained" is replaced by "after repeating step (1) for 20 times, a hollow fiber membrane modified twenty-one times is obtained"; in step (3), the hollow fiber membrane modified six times is replaced by the hollow fiber membrane modified twenty-one times in this comparative example, and other conditions remain unchanged.
[0082] Comparative Example 1
[0083] In this comparative example, the synthesized dendritic polyamidoamine was used to modify the polysulfone hollow fiber membrane with an average pore size of 50 nm, specifically according to the following steps:
[0084] 1. Preparation of dendritic polyamidoamine
[0085] (1) preparing a methanol mixed solution of 5 wt % ethylenediamine and 10 wt % methyl acrylate, reacting the mixture at 30° C. in the dark for 24 h, and then removing methanol and unreacted monomers by vacuum rotary evaporation to obtain a 0.5 generation dendritic polyamidoamine;
[0086] (2) dissolving a 0.5 generation dendritic polyamidoamine in a 10 wt % ethylenediamine methanol solution, reacting at 30° C. in the dark for 24 h, and then removing methanol and unreacted monomers by vacuum rotary evaporation to obtain a 1.0 generation dendritic polyamidoamine;
[0087] (3) dissolving the 1.0 generation dendritic polyamidoamine in a 10 wt % methanol solution of methyl acrylate, reacting at 30° C. in the dark for 24 h, and then removing methanol and unreacted monomers by vacuum rotary evaporation to obtain the 1.5 generation dendritic polyamidoamine;
[0088] (4) after repeating step (2) and step (3) for the fourth time, a 5.5-generation dendritic polyamidoamine is obtained;
[0089] 2. Amination of polysulfone hollow fiber membrane
[0090] (1) The polysulfone hollow fiber membrane is immersed in an isopropanol solution of 8 wt.% ammonium nitrate and 73.5 wt.% trifluoroacetic anhydride, and reacted at 25°C for 4 hours to complete the nitration of the polysulfone hollow fiber membrane; then immersed in an isopropanol solution of tetrabutylammonium chloride at 70°C for 12 hours to complete the amino modification, and washed with methanol for multiple times to obtain an amino polysulfone hollow fiber membrane;
[0091] 3. Preparation of modified hollow fiber membrane
[0092] (1) dissolving 5.5-generation dendritic polyamidoamine in methanol to prepare a 10 wt% solution to obtain a methanol solution of 5.5-generation dendritic polyamidoamine; immersing an aminated polysulfone hollow fiber membrane in the methanol solution of 5.5-generation dendritic polyamidoamine and reacting at 30° C. for 24 hours to obtain a polysulfone hollow fiber membrane directly modified with 5.5-generation dendritic polyamidoamine;
[0093] (2) The 5.5-generation dendritic polyamide amine directly modified polysulfone hollow fiber membrane was immersed in a 2 wt % polyacrylic acid aqueous solution and the cross-linking modification was completed at a constant temperature of 40° C. within 10 hours. After rinsing with deionized water, a cross-linked dendritic polyamide amine directly modified polysulfone hollow fiber separation membrane was obtained.
[0094] Comparative Example 2
[0095] In this comparative example, a polysulfone hollow fiber ultrafiltration membrane with an average pore size of 50 nm was modified in one step, specifically according to the following steps:
[0096] (1) Amination of polysulfone hollow fiber membrane: The polysulfone hollow fiber membrane is immersed in an isopropanol solution of 8 wt % ammonium nitrate and 73.5 wt % trifluoroacetic anhydride, and reacted at 25° C. for 4 h to complete the nitration of the polysulfone hollow fiber membrane; then immersed in an isopropanol solution of tetrabutylammonium chloride, and reacted at 70° C. for 12 h to complete the amination modification, and washed with methanol for multiple times to obtain an amination polysulfone hollow fiber membrane;
[0097] (2) placing the aminated polysulfone hollow fiber separation membrane in a mixed aqueous solution of 10 wt % N,N'-methylenebisacrylamide and 10 wt % N-aminoethylpiperazine, reacting at 30° C. for 12 h, taking out the polysulfone hollow fiber separation membrane, and repeatedly washing the unreacted monomers in the membrane and the free polymer generated by the reaction and not grafted on the membrane with deionized water to obtain a polyamideamine-modified polysulfone hollow fiber membrane;
[0098] (3) The polyamide-amine modified polysulfone hollow fiber membrane is immersed in a 2 wt % polyacrylic acid aqueous solution and the cross-linking modification is completed at a constant temperature of 40° C. within 10 hours. After being rinsed with deionized water, a cross-linked polyamide-amine modified polysulfone hollow fiber membrane is obtained, i.e., a modified hollow fiber membrane.
[0099] Comparative Example 3
[0100] The preparation method is basically the same as that of Comparative Example 2, except that the constant temperature reaction at 30° C. for 12 h in step (2) of Comparative Example 2 is replaced by a constant temperature reaction at 30° C. for 24 h, and other conditions remain unchanged.
[0101] Comparative Example 4
[0102] In this comparative example, a free radical graft polymerization method is used to hydrophilize a polysulfone hollow fiber membrane with an average pore size of 50 nm, and the specific steps are as follows:
[0103] (1) Plasma pretreatment of polysulfone hollow fiber membrane: The polysulfone hollow fiber membrane was placed in a plasma treatment instrument and treated at 50 W for 30 s under an argon atmosphere to complete the pretreatment;
[0104] (2) The pretreated polysulfone hollow fiber membrane is immediately taken out and immersed in a 10 wt % acrylamide isopropanol solution, and reacted at 40° C. for 4 h. After being taken out, it is repeatedly rinsed with ethanol and deionized water to obtain a polysulfone hollow fiber membrane modified by polyacrylamide amine grafting, i.e., a modified hollow fiber membrane.
[0105] Comparative Example 5
[0106] The preparation method is basically the same as that of Comparative Example 4, except that the constant temperature reaction at 40° C. for 4 h in step (2) of Comparative Example 4 is replaced by a constant temperature reaction at 40° C. for 8 h, and other conditions remain unchanged.
[0107] Comparative Example 6
[0108] The preparation method is basically the same as that of Example 1, except that step (2) is removed; the hollow fiber membrane modified six times in step (3) is replaced by the hollow fiber membrane modified once in this comparative example, and other conditions remain unchanged.
[0109] Test example
[0110] The performance of the modified hollow fiber membranes of the embodiments and comparative examples was characterized by the following test methods:
[0111] 1. Average pore size and pore size distribution
[0112] At room temperature of 25°C, a pore size analyzer (BSD-PBL) was used to analyze a cross section of the membrane.
[0113] 2. Determination of grafting rate
[0114] The hollow fiber membranes before and after modification were rinsed with pure water, vacuum dried and weighed, and the grafting rate of the membrane was calculated according to the formula: grafting rate (%) = (mass of modified hollow fiber membrane - mass of hollow fiber membrane before modification) / mass of modified hollow fiber membrane × 100%.
[0115] 3. Determination of water contact angle
[0116] Select a membrane product with a uniform inner and outer diameter of about 2 cm and dry it in a 60°C oven for 1 hour. Use double-sided tape to stick the dried membrane product evenly on the surface of a glass slide. Then place the glass slide on the platform of the contact angle tester and use about 0.1 μL of pure water to measure the static contact angle on the KRUSS-DSA100 contact angle tester by the drop method to obtain the water contact angle of the membrane product. Each membrane product is measured at 3 different positions, and the arithmetic average of the contact angle is taken to obtain the average contact angle of the membrane product.
[0117] 4. Determination of Zeta potential on membrane surface
[0118] A membrane product with a uniform inner and outer diameter of about 5 cm was selected and soaked in alcohol, then replaced with deionized water. The membrane was then encapsulated in a specific component and the surface Zeta potential of the membrane sample was measured using the streaming potential method on the Anton Paar-SurPASS 3 electric solid surface analyzer. Three groups of samples were taken from each group of membranes for measurement, and each sample was tested 3 times. The arithmetic average was taken to obtain the surface Zeta potential of each group of membranes.
[0119] 5. Water flux test
[0120] The hollow fiber membranes before and after modification were packaged into components and then placed in a membrane performance evaluation device for testing. The operating pressure was 0.1 MPa and the water temperature was 25°C. The water production per unit time was collected and measured. The water flux can be calculated by the following formula:
[0121]
[0122] In the formula, J w is the pure water flux, L·m -2 ·h -1 ; V is the water production per unit time, L; A is the effective filtration membrane area, m 2 ; ΔT is the test time, h.
[0123] 6. Determination of protein adsorption performance
[0124] The hollow fiber membranes before and after modification were dried at a constant temperature to determine their initial mass. After being washed with ethanol and deionized water, they were placed in a solution prepared with bovine serum albumin (BSA) (isoelectric point 4.7, negatively charged) to simulate a solution containing protein. The pH of the protein solution was adjusted to 4.7 with a phosphate buffer solution and immersed at a constant temperature of 25°C for 24 hours to allow the membrane surface and pores to fully adsorb BSA. After being rinsed with deionized water and dried, their mass was determined. The adsorption amount was obtained by the following formula:
[0125] Protein adsorption amount = (M1-M0) / A
[0126] Where, protein adsorption, μg / cm 2 ; M1 is the mass of the modified hollow fiber membrane after protein adsorption, μg; M0 is the original mass of the hollow fiber membrane before modification, μg; A is the effective area of the outer surface of the membrane, cm 2 .
[0127] 7. Determination of membrane flux attenuation rate and cleaning recovery rate
[0128] The determination was carried out through a protein solution permeation experiment, which specifically included the following steps: encapsulating the hollow fiber membranes before and after modification into a component, preparing bovine serum albumin (BSA) into a solution to simulate a solution containing protein, and adjusting the pH of the protein solution to 4.7 with a phosphate buffer solution. Under the conditions of an operating pressure of 0.1 MPa and an operating temperature of 25°C, the protein solution was pressed into the hollow fiber membrane component, and the mass of the permeate was collected and measured every 10 minutes, and the membrane flux attenuation rate was calculated by the following formula:
[0129] F=(1-J f / J w )×100%
[0130] Where, F is the flux attenuation rate of the membrane, %; J f Water flux for real-time BSA testing, L·m -2 ·h -1 ; J w is the pure water flux, L·m -2 ·h -1 .
[0131] The membrane was washed with 0.01 mol / L NaOH solution and deionized water for 30 min, and then the pure water flux of the membrane was tested, which was recorded as J w1 , the membrane flux recovery rate RFR (%) can be calculated by the following formula:
[0132] RFR=J w1 / J w ×100%
[0133] Table 1 Performance characterization results of modified hollow fiber membrane
[0134]
[0135] According to Table 1, we can see that:
[0136] 1. By comparing Examples 1-13 and Comparative Examples 1-6 as well as polysulfone hollow fiber membranes and polyethersulfone hollow fiber membranes, it can be seen that the method of the present invention can achieve hydrophilic modification of the hollow fiber membrane, and the membrane flux attenuation after modification is less than 15%, while having high pure water flux, low protein adsorption, low flux attenuation rate and high cleaning recovery rate.
[0137] 2. By comparing Examples 1-3 and Examples 11-13, it can be seen that the present invention can achieve regulation of the number of surface modification layers and the grafting rate by controlling the number of repeated executions, thereby achieving regulation of the average pore size of the membrane.
[0138] 3. Comparative Examples 4-7 show that the Zeta potential of the surface of the modified hollow fiber membrane can be regulated by controlling the type and concentration of the cross-linking agent, which is beneficial to the adsorption of different proteins.
[0139] 4. By comparing Examples 1-11 and Examples 12-13, it can be seen that as the grafting rate increases, the water flux may decrease, but low protein adsorption, low flux attenuation rate and high cleaning recovery rate can still be guaranteed.
[0140] 5. By comparing Examples 1-13 and Comparative Examples 1-6, it can be seen that the in-situ grafting modification and stepwise synthesis methods adopted in the present invention have better controllability of the grafting rate and average pore size of the membrane compared to synthesizing dendritic polymers first and then grafting them, one-step grafting modification, and free radical polymer grafting methods, and improve the membrane's pollution resistance while ensuring low flux attenuation rate and high cleaning recovery rate. The inventor believes through research that during one-step grafting modification, there are reactions of alkenyl grafting amine monomers and amine grafting alkenyl monomers, which easily lead to longer chain segment growth; if dendritic polymers are synthesized first and then grafted, it is easy to cause some sites to be grafted, but other sites are not grafted, which ultimately leads to greater steric hindrance and a decreased grafting rate, which is not conducive to the improvement of membrane performance.
[0141] according to Figure 1 , Figure 2 , Figure 3 From the SEM image, it can be seen that the surface pore size and position distribution of the modified hollow fiber membrane prepared by the present invention are more uniform. The inventor speculates that when the dendritic polymer is directly grafted, the grafting is mainly carried out on the membrane surface, resulting in a significant reduction in the pore size of some positions on the membrane surface, which in turn leads to a significant decrease in the pure water flux of the membrane. In this application, the compounds added by gradual reaction are all small molecular compounds, which are easy to diffuse into the pores. In addition, by controlling the monomer concentration and reaction time, it is ensured that the monomers can fully diffuse into the pores; Comparative Example 1 is to graft the synthesized dendritic polymer onto the membrane. Due to the large molecular weight and volume of the polymer, it is not easy to enter the membrane pores. It is basically carried out on the membrane surface, resulting in a reduction in pore size and even pore blockage.
[0142] according to Figure 4 It can be seen that the pore size distribution of the modified hollow fiber membrane prepared by the modification method of the present invention is uniform, and the modification has little effect on the pore size distribution of the fiber membrane itself, which can minimize the influence of the grafted modified molecules on the pore size distribution of the membrane itself. The inventor believes through research that grafting is the growth of polymers on the membrane surface and the pore wall surface. Only when the grafting (growth) is uniform, all surfaces grow uniformly to a certain thickness (<1nm) to ensure uniform pore size; if the grafting is uneven, it will lead to a reduction in some pore sizes, and may even cause clogging of the membrane pores.
[0143] The preferred specific embodiments and experimental verification of the present invention are described in detail above. It should be understood that ordinary technicians in this field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in this technical field based on the concept of the present invention through logical analysis, reasoning or limited experiments on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A controllable modification method for improving the hydrophilicity of a hollow fiber membrane, characterized in that: The following steps are involved: (1) placing an aminated hollow fiber membrane raw material in a solution containing an olefin monomer, reacting at 10-70° C. for 1-24 hours to obtain a fiber membrane intermediate; The fiber membrane intermediate is placed in a solution containing a polyamine monomer, and reacted at 10-70° C. for 1-24 hours to obtain a primary modified hollow fiber membrane; (2) using the once modified hollow fiber membrane as a raw material, repeating step (1) once to obtain a modified hollow fiber membrane; (3) cross-linking the modified hollow fiber membrane; The cross-linking treatment comprises: placing the modified hollow fiber membrane in a solution containing a cross-linking agent for reaction at 20-70° C.; the cross-linking agent comprises at least one of polyacrylic acid, polymethacrylic acid, polystyrene sulfonic acid, and polyvinyl sulfonic acid; Wherein, the olefinic monomer includes at least one of methyl acrylate, ethyl acrylate, propyl acrylate, acrylamide, N-ethylacrylamide, N,N'-methylenebisacrylamide, and N-propylacrylamide; The polyamine monomer includes at least one of ethylenediamine, propylenediamine, 1,2,3-propylenetriamine, diethylenetriamine, and N-aminoethylpiperazine; The concentration of the olefinic monomer in the solution containing the olefinic monomer is 0.1-30 wt %, and the volume ratio of the solution containing the olefinic monomer to the aminated hollow fiber membrane raw material is (2:1)-(100:1); The concentration of the polyamine monomer in the solution containing the polyamine monomer is 0.1-30 wt %, and the volume ratio of the solution containing the polyamine monomer to the aminated hollow fiber membrane raw material is (2:1)-(100:1).
2. The controllable modification method according to claim 1, characterized in that: After step (2), the method further comprises: repeating step (1) on the modified hollow fiber N times, where 1≤N≤19.
3. The controllable modification method according to claim 1 or 2, characterized in that: The mass ratio of the olefin monomer to the polyamine monomer is (1:3)-(3:1).
4. The controllable modification method according to claim 1, characterized in that: The grafting rate of the modified hollow fiber membrane is 3-20%.