A kind of petroleum fracturing proppant and preparation method thereof
The petroleum fracturing proppant prepared by combining hollow glass beads and slag powder with epoxy resin solves the problems of high proppant density and difficult construction in the existing technology, and achieves low density, high strength and strong anti-fragmentation ability. The effect is to simplify the fracturing construction process.
Patent Information
- Application Number
- CN202211553430.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-06
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-06
AI Technical Summary
Existing petroleum fracturing proppant has a high density, which makes construction difficult and inconvenient to pump downhole, and requires the use of high-molecular viscous fracturing fluid.
Hollow glass beads and slag powder are used as support materials, combined with epoxy resin to prepare petroleum fracturing proppant, and are made into spherical particles through graft modification and molding equipment to reduce density and improve strength and anti-fragmentation ability.
Obtain petroleum fracturing proppant with low density, high strength and strong anti-fracture ability, which can directly use water as fracturing fluid, simplify the construction process and reduce the use of fracturing fluid.
Smart Images

Figure BDA0003982016070000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of petroleum proppants, and in particular, relates to a petroleum fracturing proppant and a preparation method thereof. Background Art
[0002] In oil and gas production in oil fields, fracturing technology is widely used to increase oil well production, extend the high-yield life of oil wells, and exploit difficult-to-use resources. In order to prevent the closure of underground fractures, retain oil and gas channels, and maintain conductivity, proppants must be used to fill the cracks. Petroleum proppants are also called petroleum fracturing proppants. In deep well oil and gas production, high closure pressure and low permeability deposits are treated by fracturing to crack the oil and gas-bearing rock formations, and oil and gas are collected from the channels formed by the cracks. At this time, fluid needs to be injected into the rock base to exceed the pressure of the formation fracture strength, so that cracks are generated in the rock formations around the wellbore, forming a channel with high-level flow capacity, in order to keep the cracks formed after fracturing open, so that oil and gas products can pass smoothly.
[0003] In recent years, with the development of domestic oil fracturing proppants, proppants are no longer limited to the two conventional types of quartz sand and ceramsite. Various proppants have emerged, such as coated proppants, consolidable proppants, and selective oil-permeable and water-blocking proppants. The conductivity of resin-coated proppants is better than that of quartz sand and ceramsite. This is mainly because the outer layer of coated resin wraps the crushed quartz sand and ceramsite inside to prevent the broken fine particles from blocking the crack channel and reducing the conductivity. However, resin-coated proppants generally use materials such as quartz sand or ceramics with higher density, which makes the density of fracturing proppants still relatively high. It is necessary to use high-molecular viscous fracturing fluid to press and export it, which undoubtedly causes construction difficulties and is not convenient for pumping into the well. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a petroleum fracturing proppant and a preparation method thereof.
[0005] The present invention uses hollow glass microspheres and slag micropowder as propping materials and prepares petroleum fracturing propping agents together with epoxy resin to obtain a product with low density, high strength and strong anti-crushing ability. The petroleum fracturing propping agent obtained by the present invention has low density, so no or less polymer fracturing fluid can be used, and water can be directly used as fracturing fluid for transportation, thereby reducing the use of fracturing fluid and simplifying the fracturing construction process.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A method for preparing a petroleum fracturing proppant comprises the following steps:
[0008] The first step is to mix the hollow glass microspheres and the slag micropowder, soak them in alkali solution for 8-10 minutes, take them out, wash them with water until they are neutral, dry them, and then use silane coupling agent KH792 to graft and modify their surfaces to obtain pre-treated support materials;
[0009] The second step is to react the pretreated support material with chloropolyethylene glycol to obtain a modified support material;
[0010] Step 3: Mix the epoxy resin with the curing agent, accelerator, toughening agent and modified support material in proportion and disperse them evenly to obtain epoxy resin mixed glue;
[0011] Step 4: Heat the methyl silicone oil to 140-150°C for use; use a molding device to make the epoxy resin mixed glue into spherical particles, then drip the heated methyl silicone oil into it to solidify it for 0.5-1h, then cool it to room temperature, wash it with toluene and petroleum ether, filter it, separate it, and dry it to obtain an oil fracturing proppant.
[0012] Furthermore, in the first step, the specific process of grafting modification with silane coupling agent KH792 is as follows:
[0013] The dried powder was mixed with an ethanol aqueous solution (volume fraction of 50%) at a ratio of 1 g: 15 mL, ultrasonically dispersed for 10 min, and then the silane coupling agent KH792 was added. The temperature was raised to 80° C., stirred and refluxed for 4-5 h, filtered, washed with distilled water 3-4 times, and fully dried to obtain a pretreated support material; the amount of silane coupling agent KH792 added was 2-3 times the mass of the powder.
[0014] Furthermore, the specific operation of the second step is: dissolving chloropolyethylene glycol in DMF at a mass ratio of 1:9, mixing and dissolving evenly, and then mixing with the pretreated support material at a solid-liquid ratio of 1g:20mL, stirring for 4-5h, filtering, washing with ethanol 3-4 times, and fully drying to obtain a modified support material; the surface of the pretreated support material is grafted with a molecular chain of a silane coupling agent KH792, and the -NH 2 It can react with chloropolyethylene glycol, thereby grafting polyethylene glycol molecular chains on its surface to obtain a modified support material.
[0015] Furthermore, the particle size of the slag powder is 15-25 μm.
[0016] Furthermore, in the first step, the alkali solution is any one of a sodium hydroxide solution, a potassium hydroxide solution and a calcium hydroxide solution, and the pH value of the alkali solution is 10-12.
[0017] Furthermore, the viscosity of the methyl silicone oil is 10 Pa·s; the curing agent is curing agent MTHPA, the accelerator is accelerator DMP-30, and the toughening agent is polytetrahydrofuran toughening agent PTMG3000.
[0018] Furthermore, the usage ratio of epoxy resin, curing agent, accelerator, toughening agent, modified support material and methyl silicone oil is 100g:80-85g:2-3g:5-6g:7-10g:3000mL.
[0019] Furthermore, the mass ratio of the hollow glass microspheres to the slag micropowder is 3:2.
[0020] The modified support material is prepared by modifying hollow glass microspheres and slag micropowder; in addition to ultra-low density, the hollow glass microspheres have the characteristics of high compressive strength, high melting point, high resistivity, small thermal conductivity and thermal shrinkage coefficient. Using them as one of the support materials can obtain higher anti-crushing ability; the slag micropowder has a small particle size, and the slag itself has the advantages of high temperature resistance and high strength, which can also improve the comprehensive performance of the proppant; and the surface of the modified support material is grafted with polyethylene glycol molecular chains, which, on the one hand, can improve the interface compatibility between the support material and the epoxy resin, thereby improving the dispersion performance; on the other hand, an interpenetrating polymerization network will be formed between the flexible polyethylene glycol molecular chains and the epoxy resin molecular chains, further enhancing the carrying and dispersion capabilities of the support material, thereby ensuring that the final prepared microspheres have high strength and excellent sphericity.
[0021] Beneficial effects of the present invention:
[0022] The present invention uses hollow glass microspheres and slag micropowder as propping materials and prepares petroleum fracturing propping agents together with epoxy resin to obtain a product with low density, high strength and strong anti-crushing ability. The petroleum fracturing propping agent obtained by the present invention has low density, so no or less polymer fracturing fluid can be used, and water can be directly used as fracturing fluid for transportation, thereby reducing the use of fracturing fluid and simplifying the fracturing construction process. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Example 1
[0025] A method for preparing a petroleum fracturing proppant comprises the following steps:
[0026] Step 1: Mix 60g of hollow glass microspheres and 40g of slag powder (particle size 15-25μm), soak them in sodium hydroxide solution (pH 10) for 8min, take them out, wash them with water until neutral, and dry them;
[0027] The dried powder was mixed with an ethanol aqueous solution (volume fraction 50%) at a ratio of 1 g: 15 mL, ultrasonically dispersed for 10 min, and then a silane coupling agent KH792 was added, the temperature was raised to 80° C., stirred and refluxed for 4 h, filtered, washed with distilled water for 3 times, and fully dried to obtain a pretreated support material; the amount of the silane coupling agent KH792 added was twice the mass of the powder;
[0028] Step 2: Dissolve chloropolyethylene glycol in DMF at a mass ratio of 1:9, mix and dissolve evenly, then mix with the pretreated support material at a solid-liquid ratio of 1g:20mL, stir for 4h, filter, wash with ethanol 3 times, and fully dry to obtain a modified support material;
[0029] Step 3: Mix 1kg of epoxy resin with 800g of curing agent MTHPA, 20g of accelerator DMP-30, 50g of polytetrahydrofuran toughening agent PTMG3000, and 70g of modified support material in proportion, disperse evenly, and obtain epoxy resin mixed glue;
[0030] Step 4: Heat 30L of methyl silicone oil to 140°C and set aside; use a molding device to make the epoxy resin mixed glue into spherical particles, then drip the heated methyl silicone oil (viscosity of 10Pa·s) into it to solidify it for 0.5h, then cool it to room temperature, wash it with toluene and petroleum ether, filter it, separate it, and dry it to obtain an oil fracturing proppant.
[0031] Example 2
[0032] A method for preparing a petroleum fracturing proppant comprises the following steps:
[0033] Step 1: Mix 60g of hollow glass microspheres and 40g of slag powder (particle size 15-25μm), soak them in potassium hydroxide solution (pH 11) for 9 minutes, take them out, wash them with water until neutral, and dry them;
[0034] The dried powder was mixed with an ethanol aqueous solution (volume fraction of 50%) at a ratio of 1 g: 15 mL, and ultrasonically dispersed for 10 min, and then a silane coupling agent KH792 was added, the temperature was raised to 80° C., and the mixture was stirred and refluxed for 4.5 h. The mixture was filtered, washed with distilled water for 4 times, and fully dried to obtain a pretreated support material; the amount of the silane coupling agent KH792 added was 2.5 times the mass of the powder;
[0035] Step 2: Dissolve chloropolyethylene glycol in DMF at a mass ratio of 1:9, mix and dissolve evenly, then mix with the pretreated support material at a solid-liquid ratio of 1g:20mL, stir for 4.5h, filter, wash with ethanol 4 times, and fully dry to obtain a modified support material;
[0036] Step 3: Mix 1kg of epoxy resin with 825g of curing agent MTHPA, 25g of accelerator DMP-30, 55g of polytetrahydrofuran toughening agent PTMG3000, and 85g of modified support material in proportion, and disperse them evenly to obtain epoxy resin mixed glue;
[0037] Step 4: Heat 30L of methyl silicone oil to 145°C for use; use a molding device to make the epoxy resin mixed glue into spherical particles, then drip the heated methyl silicone oil (viscosity of 10Pa·s) into it to solidify it for 45 minutes, then cool it to room temperature, wash it with toluene and petroleum ether, filter it, separate it, and dry it to obtain an oil fracturing proppant.
[0038] Example 3
[0039] A method for preparing a petroleum fracturing proppant comprises the following steps:
[0040] Step 1: Mix 60g of hollow glass microspheres and 40g of slag powder (particle size 15-25μm), soak them in calcium hydroxide solution (pH 12) for 10min, take them out, wash them with water until neutral, and dry them;
[0041] The dried powder was mixed with an ethanol aqueous solution (volume fraction 50%) at a ratio of 1 g: 15 mL, ultrasonically dispersed for 10 min, and then a silane coupling agent KH792 was added, the temperature was raised to 80° C., stirred and refluxed for 5 h, filtered, washed with distilled water 4 times, and fully dried to obtain a pretreated support material; the amount of the silane coupling agent KH792 added was 3 times the mass of the powder;
[0042] Step 2: Dissolve chloropolyethylene glycol in DMF at a mass ratio of 1:9, mix and dissolve evenly, then mix with the pretreated support material at a solid-liquid ratio of 1g:20mL, stir for 4-5h, filter, wash with ethanol 4 times, and fully dry to obtain a modified support material;
[0043] Step 3: Mix 1kg of epoxy resin with 850g of curing agent MTHPA, 30g of accelerator DMP-30, 60g of polytetrahydrofuran toughening agent PTMG3000, and 100g of modified support material according to proportion, and disperse them evenly to obtain epoxy resin mixed glue;
[0044] Step 4: Heat 30L of methyl silicone oil to 150°C and set aside; use a molding device to make the epoxy resin mixed glue into spherical particles, then drip the heated methyl silicone oil (viscosity of 10Pa·s) into it to solidify it for 1 hour, then cool it to room temperature, wash it with toluene and petroleum ether, filter it, separate it, and dry it to obtain an oil fracturing proppant.
[0045] The performance test of the petroleum cracking proppant prepared in Examples 1-3 was carried out, and the test results are shown in the following table:
[0046]
[0047] It can be seen from the data in the above table that the petroleum fracturing proppant obtained by the present invention has the advantages of low density, high strength, strong anti-crushing ability, etc.
[0048] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0049] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a petroleum fracturing proppant, characterized in that: The steps include: The first step is to mix hollow glass microspheres and slag micropowder in a mass ratio of 3:2, soak them in alkali solution for 8-10 minutes, take them out, wash them with water until they are neutral, dry them, and then use silane coupling agent KH792 to graft and modify their surfaces to obtain pretreated support materials; The second step is to react the pretreated support material with chloropolyethylene glycol to obtain a modified support material; The surface of the pretreated support is grafted with a molecular chain of a silane coupling agent KH792, and the -NH2 contained therein can react with chloropolyethylene glycol, thereby grafting a polyethylene glycol molecular chain on the surface thereof to obtain a modified support; Step 3: Mix the epoxy resin with the curing agent, accelerator, toughening agent and modified support material in proportion and disperse them evenly to obtain epoxy resin mixed glue; Step 4: Heat the methyl silicone oil to 140-150°C for standby use; use a molding device to make the epoxy resin mixed glue into spherical particles, then drip the heated methyl silicone oil into it to solidify it for 0.5-1h, then cool it to room temperature, wash it with toluene and petroleum ether, filter it, separate it, and dry it to obtain an oil fracturing proppant; In the above steps, the usage ratio of epoxy resin, curing agent, accelerator, toughening agent, modified support material and methyl silicone oil is 100g:80-85g:2-3g:5-6g:7-10g:3000mL.
2. The method for preparing a petroleum fracturing proppant according to claim 1, characterized in that: In the first step, the specific process of grafting modification with silane coupling agent KH792 is as follows: The dried powder was mixed with ethanol aqueous solution at a ratio of 1 g:15 mL, ultrasonically dispersed for 10 min, and then added with silane coupling agent KH792. The temperature was raised to 80° C., stirred and refluxed for 4-5 h, filtered, washed with distilled water for 3-4 times, and fully dried to obtain a pretreated support material.
3. The method for preparing a petroleum fracturing proppant according to claim 2, characterized in that: The amount of silane coupling agent KH792 added is 2-3 times the mass of the powder.
4. The method for preparing a petroleum fracturing proppant according to claim 1, characterized in that: The specific operation of the second step is: dissolve chloropolyethylene glycol in DMF at a mass ratio of 1:9, mix and dissolve evenly, then mix with the pretreated support material at a solid-liquid ratio of 1g:20mL, stir for 4-5h, filter, wash with ethanol 3-4 times, and fully dry to obtain a modified support material.
5. The method for preparing a petroleum fracturing proppant according to claim 1, characterized in that: The particle size of the slag powder is 15-25 μm.
6. The method for preparing a petroleum fracturing proppant according to claim 1, characterized in that: In the first step, the alkali solution is any one of a sodium hydroxide solution, a potassium hydroxide solution and a calcium hydroxide solution, and the pH value of the alkali solution is 10-12.
7. The method for preparing a petroleum fracturing proppant according to claim 1, characterized in that: The viscosity of methyl silicone oil is 10Pa•s; the curing agent is curing agent MTHPA, the accelerator is accelerator DMP-30, and the toughening agent is polytetrahydrofuran toughening agent PTMG3000.
8. A petroleum fracturing proppant, characterized in that: Prepared according to the method according to any one of claims 1 to 7.