A 100mm-400mm thick ultra-large specification high-strength and tough homogeneous target plate and its production method
By rationally designing chemical composition and preparation technology in large-thick homogeneous steel plates, the problems of domestic large-thick homogeneous target plate technical requirements and market demands have been solved, and high-strength, toughness and uniform steel plate production has been achieved, filling the imported targets The blank of the board provides favorable conditions for the development of national defense science and technology.
Patent Information
- Application Number
- CN202211499358.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-11-28
AI Technical Summary
It is difficult for the domestic system to meet the technical requirements and market demands of large-thick homogeneous target plates, resulting in dependence on imported target plates and the inability to achieve independent research and development and production controllability.
The chemical composition and preparation process of 100mm-400mm thick high-strength homogeneous steel plates are adopted, including iron pretreatment, smelting, casting, heating, rolling, quenching, tempering and flaw detection, through Cr, Mo, Ni, Nb, V, B The rational design of other elements can achieve high strength, toughness and uniformity of steel plates, and adopt technical means such as low-speed, large-pressure technology and sink quenching.
The steel plate with excellent strength, toughness and uniformity was obtained, filling the gap in domestic large-thick shell target plates, creating favorable conditions for the development of national defense science and technology, and achieving the purpose of replacing imported target plates.
Smart Images

Figure HDA0003966520490000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron-based alloys, and in particular relates to a thick, high-strength and tough homogeneous steel plate and a production method thereof. Background Art
[0002] Artillery shells are the main weapons and ammunition used in the world today. Armor-piercing shells are a type of shells with relatively great power and are important weapons against armored targets. The main function of the target plate is to test the armor-piercing ability of the warhead through target shooting tests. The material must have a certain strength and toughness, and high uniformity requirements. Among them, the target plate with large thickness specifications is mainly used to test the armor-piercing ability of armor-piercing shells.
[0003] With the development of cutting-edge technology in military weapons, China's armor-piercing projectiles have reached internationally advanced levels, so the demand for artillery shell target plates is increasing. Since the research and development of thick target plates in my country cannot meet the technical indicators of advanced projectile testing and the growing market demand, domestic thick target plates for artillery shells rely heavily on imports, and the independent research and development and controllable production of thick homogeneous target plates has not yet been truly realized. Summary of the invention
[0004] The present application is implemented to meet the domestic technical requirements for thick homogeneous target plates, and provides a 100-400mm thick high-strength and tough homogeneous target plate and a preparation process thereof.
[0005] The technical solution adopted by the present invention to solve the above problems is: a 100mm-400mm thick ultra-large specification high-strength and tough homogeneous target plate, the chemical composition of the target plate is calculated by mass percentage, C: 0.20-0.35%, Si: 0.15-0.40%, Mn: 0.30-0.70%, Cr: 1.80-2.60%, Mo: 0.28-0.50%, Ni: 2.50-3.50%, Al: 0.01 5~0.080%, Cu: ≤0.25%, Nb: 0.01~0.05%, V: 0.02~0.08%, B: 0.001~0.005%, Ca: 0.001~0.005%, P: ≤0.012%, S: ≤0.005%, O: ≤0.002%, N: ≤0.008%, H: ≤0.0002%, W: ≤0.13%, the balance is Fe and unavoidable impurity elements.
[0006] Furthermore, the target plate of the present application has a uniform tempered troostite structure. The target plate meets the following requirements: yield strength>600MPa, tensile strength>800MPa, elongation≥15%, and cross-sectional shrinkage≥50%; 20℃ Charpy impact energy≥120J, -40℃ Charpy impact energy≥70J; fracture surface is tested according to GJB31A-2000 standard, with no white spots, fibrous grade 1-2, slate grade 1-2, and stratified grade 1-2; and the steel plate is tested according to GB / T2970-2016 standard, meeting the requirements of grade I.
[0007] The fracture detection of the target plate helps to evaluate the plasticity and toughness of the material.
[0008] The reasons why the present invention adopts the above-mentioned components and their weight percentages are described in detail below:
[0009] C: The C element can improve the strength and hardness of the steel plate, but in order to ensure the low-temperature impact toughness of the material, it is necessary to limit the upper and lower limits. The C content of the present invention is controlled at 0.20-0.35%.
[0010] Si: Si element can play a deoxidizing role in steel and can improve the hardness of the material by being dissolved in austenite, but too high Si element will be detrimental to the plasticity of the steel. In the present invention, the Si content is controlled at 0.15-0.40%.
[0011] Mn: Mn can improve the strength and hardenability of materials, but too high a content of Mn will increase the center segregation of thick plates. In the present invention, the Mn content is controlled at 0.30-0.70%.
[0012] Cr: Cr element can form Cr carbide with C, improve hardenability, improve steel strength, hardness, wear resistance, and improve high temperature mechanical properties of steel plate, and improve steel oxidation resistance and corrosion resistance. The Cr content of the present invention is controlled at 1.80-2.60%.
[0013] Mo: Mo element exists in the form of solid solution and carbide in steel, which can improve the strength and hardenability of steel plate. Mo is used in combination with Cr and Mn elements to improve the tempering stability of steel. The Mo content of the present invention is controlled at 0.28-0.50%.
[0014] Ni: Ni is a strengthening element in steel. It exists in the steel in the form of solid solution and can improve the strength and hardenability of the steel. As the Ni content increases, the strength of the steel increases without significantly reducing the plasticity and toughness. At the same time, the Ni element can effectively improve the low-temperature toughness of the steel. The Ni content of the present invention is controlled at 2.50-3.50%.
[0015] Nb: Nb can refine grains, reduce overheat sensitivity and temper brittleness of steel, and improve strength. The Nb content of the present invention is controlled at 0.01-0.05%.
[0016] V: V is a carbonitride forming element, which can improve the strength and toughness of steel through dispersion strengthening and refine grains. The V content of the present invention is controlled at 0.02-0.08%.
[0017] B: The main function of B in steel is to increase the hardenability of steel and improve the performance of steel plates after quenching and tempering. The content of B in the present invention is controlled at 0.001-0.005%.
[0018] N and H are harmful elements in the steel of the present invention, which may cause processing cracks, and should be controlled as low as possible.
[0019] P and S are harmful elements in the steel of the present invention, which will reduce the quality of the steel plate and should be controlled as low as possible.
[0020] The effect of the above alloy elements is: through the reasonable design of Cr, Mo, Ni, Nb, V, B and other elements, the composite strengthening effects such as solid solution strengthening and fine grain strengthening are fully exerted to improve the strength, toughness and performance uniformity of the steel plate. The final steel plate and the cut target plate have great advantages in thickness and excellent homogeneity and density.
[0021] Another object of the present invention is to provide a method for producing a 100mm-400mm thick ultra-large specification high-strength and tough homogeneous target plate, the specific preparation process flow is: molten iron pretreatment - smelting - pouring - heating - rolling - quenching - tempering - flaw detection - cutting and printing.
[0022] Specifically include:
[0023] Step 1, molten steel smelting: smelt molten steel according to the chemical composition of the target plate. In order to ensure the uniformity of the performance of the steel plate target plate, strict requirements are placed on the gas content in the molten steel, O≤13ppm, H≤2.0ppm, N≤50ppm;
[0024] Step 2: Pouring: Using the die casting process, the molten steel is cast into a flat steel ingot with a thickness of ≥780mm and a single weight of ≥35 tons. After the steel ingot is demoulded, it is slowly cooled for more than 24 hours. After the steel ingot is slowly cooled, it is cleaned with warm water at a cleaning temperature of ≥200℃.
[0025] Step 3, heating: the steel ingot is heated to 1230-1260℃;
[0026] Step 4, rolling: adopt low-speed large reduction process, the rolling speed is controlled at 1.0-1.5m / s, the first 4 passes use the high-temperature austenite recrystallization stage of the slab, set the reduction of each pass to 40-60mm, for the production thickness>200mm steel plate, no warm rolling, that is, no controlled rolling, directly rolled to the final plate thickness, the final rolling temperature ≥900℃; for the production thickness ≤200mm steel plate, the warm thickness is 1.5-2.0 times the finished product thickness, the start rolling temperature is 850~900℃, the final rolling temperature is 800~850℃; the steel plate rolling reduction ratio is ≥5; after rolling, the steel plate is slowly cooled off the line, the off-line temperature is ≥400℃, and the slow cooling time is ≥48h;
[0027] Step 5, offline quenching: quenching heating temperature 860-900℃, holding time 2.0-2.5min / mm, steel plates with a thickness of less than 150mm are heated and held, and then quickly water-cooled to below the martensitic phase transformation point, and the steel plate leaving water temperature is controlled to be 50-70℃, and then the target temperature is returned to 50-80℃, and then air-cooled to room temperature; steel plates with a thickness greater than 150mm are heated and held, and then quickly put into water, and the water cooling time is 120-150min, and quenched to room temperature;
[0028] Step 6: Tempering: heating temperature 650℃-680℃, holding time 3.5-4min / mm*steel plate thickness mm, cooling to room temperature after holding;
[0029] Step 7: Flaw detection: perform flaw detection on the steel plate according to GB / T2970-2016 standard, and the quality grade should meet the requirements of Grade I;
[0030] Step 8: Cutting and printing: According to the order requirements, use appropriate cutting methods to process the steel plate into the required homogeneous target plate size and print the mark.
[0031] Preferably, in step one, molten steel smelting includes KR molten iron pretreatment, primary smelting, LF refining, and vacuum degassing, wherein S is ≤0.003% after the KR molten iron pretreatment, and the alloy content in the molten steel is adjusted and deoxidized during the LF refining process. The high vacuum time in the vacuum degassing stage is ≥15min, and the vacuum degree of the vacuum chamber is set to <133Pa.
[0032] Preferably, in step 2, low superheat argon is used to protect the casting during the entire casting process, the superheat is controlled at 25-45°C, and the steel ingot is placed in a slow cooling pit or covered for slow cooling.
[0033] Preferably, in step five, the quenching heating of steel plates with a thickness of less than 150 mm is carried out in a continuous furnace, and after heating and heat preservation, they are quickly water-cooled in a quenching machine; steel plates with a thickness of more than 150 mm are heated in a trolley furnace and quenched in a water tank.
[0034] Preferably, in step six, tempering heating of steel plates with a thickness of less than 150 mm is carried out in a continuous furnace, and tempering of steel plates with a thickness of more than 150 mm is carried out in a trolley furnace.
[0035] Preferably, in order to reduce the segregation in the structure, the steel plate is subjected to normalizing heat treatment before the quenching treatment in step five, the normalizing heating temperature is 880-900° C., the holding time is 1.8-2.5 min / mm, and then air-cooled.
[0036] Preferably, in order to improve the flaw detection quality of the steel plate surface and core, the steel ingot is cobbled before the rolling step, and the reduction rate of the cobbling is 50%-60%.
[0037] Compared with the prior art, the present invention has the following outstanding advantages:
[0038] The 100-400 mm thick high-strength and tough homogeneous target plate of the present invention achieves higher product quality and excellent product performance, can replace imported target plates, fills the gap in domestic large-thickness artillery shell target plates, and creates favorable conditions for the development of my country's national defense science and technology.
[0039] The target plate production method of the present invention adopts a single-frame low-speed large-reduction process, and the steel plate with a thickness of more than 200 mm is not subjected to warm rolling. High-temperature uncontrolled rolling is helpful to achieve the welding of core defects of the blank; the warm thickness of the steel plate with a thickness of ≤200 mm is 1.5-2.0 times the thickness of the finished product, the compression ratio of the steel plate in this thickness range is ≥5, the core quality is guaranteed, and warm rolling is helpful to refine the material structure, thereby improving the comprehensive performance of the material.
[0040] The target plate production method of the present invention is that the steel plate with a thickness of less than 150 mm is quickly water-cooled to below the martensitic phase transformation point in the quenching machine, and the target temperature of the steel plate is returned to 50-80°C after the steel plate is discharged from the water, and then air-cooled to room temperature. Appropriate temperature return helps to relieve the stress of the quenched steel plate, and can increase the proportion of residual austenite in the structure, which helps to improve the toughness of the material. Steel plates with a thickness greater than 150 mm are quenched in a water tank, and are quickly put into water after heating and heat preservation. The water cooling time is 120-150 minutes. Due to the large thickness of the steel plate, the steel plate needs to be quenched to room temperature to improve the hardening effect. The metallographic structure of the target plate in the thickness direction is uniform tempered troostite. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a physical picture of the target plate of the present invention. DETAILED DESCRIPTION
[0042] The present invention is further described in detail below in conjunction with examples. The examples are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0043] Example 1
[0044] The chemical composition of the 320mm thick high-strength and tough homogeneous target plate is: C: 0.31%, Si: 0.23%, Mn: 0.45%, Cr: 2.35%, Mo: 0.45%, Ni: 2.80%, Al: 0.025%, Cu: 0.05%, Nb: 0.02%, V: 0.05%, B: 0.0020%, Ca: 0.0025%, P: 0.010%, S: 0.003%, O: 0.0018%, N: 0.0053%, H: 0.00013%, W: 0.013%, and the balance is Fe and unavoidable impurity elements.
[0045] The preparation process of 320mm thick high-strength and tough homogeneous target plate is as follows:
[0046] (1) Hot metal pretreatment: Hot metal is pretreated by KR and deep desulfurization is performed, and the sulfur content is 0.002% at the end of the treatment.
[0047] (2) Smelting. A 100-ton converter is used for smelting, and the molten steel is alloyed when tapping. Then, the LF furnace is refining for 47 minutes. The composition and temperature of the molten steel are adjusted in the LF furnace, and deoxidizer is added for deoxidation. Then, vacuum degassing is carried out at RH, with a vacuum degree of 68Pa and a high vacuum time of 15 minutes to reduce the gas content.
[0048] (3) Pouring. The die casting process is adopted, and low superheat argon is used to protect the pouring throughout the process. The superheat is controlled at 25-40℃, and the molten steel is cast into a 45-ton flat steel ingot with a thickness of 970mm. After the steel ingot is demolded, it is placed in a slow cooling pit for 48 hours. After the steel ingot is removed from the pit, it is cleaned with warm water at a cleaning temperature of 230℃.
[0049] (4) Heating: The steel ingot is heated in a soaking furnace at a soaking temperature of 1230-1260°C.
[0050] (5) Rolling. A single-stand low-speed large reduction process is adopted, and the rolling speed is controlled at 1.0-1.5 m / s. The single-pass reduction rate is increased as much as possible. The first four passes utilize the high-temperature austenite recrystallization stage of the slab, and the reduction amount of each pass is 50-60 mm. The steel plate is not rolled at warm temperature, and the final rolling temperature is 920°C. The steel plate rolling reduction ratio is ≥3. After rolling, the steel plate is put into the slow cooling pit off the line, the off-line temperature is 500°C, and the slow cooling time is 48h.
[0051] (6) Quenching. The steel plate is heated in a trolley furnace at 880°C and held for 2.5 min / mm. After heating and holding, it is quickly hoisted into a water tank for 150 min of water cooling and quenched to room temperature.
[0052] (7) Tempering. The steel plate is tempered in a trolley furnace with a heating temperature of 650℃-680℃ and a holding time of 4min / mm, followed by air cooling to room temperature.
[0053] (8) NDT. The steel plates are tested according to GB / T2970-2016, and the quality grade of the steel plates meets the I grade standard.
[0054] (9) Cutting and printing: According to the order requirements, use plasma cutting to cut the steel plate into the homogeneous target plate size required by the order, and print the mark.
[0055] The properties of the high-strength and tough homogeneous target plate produced using the above process and method are as follows:
[0056] Yield strength 675MPa, tensile strength 829MPa, elongation 16%, cross-sectional shrinkage 52%; 20℃ Charpy impact energy 143J, -40℃ Charpy impact energy 86J, fracture test results are fibrous 1, slate 2, stratified 1. The metallographic structure in the thickness direction of the target plate is uniform tempered troostite.
[0057] Example 2
[0058] The chemical composition of the 220mm thick high-strength and tough homogeneous target plate is: C: 0.28%, Si: 0.29%, Mn: 0.42%, Cr: 2.25%, Mo: 0.45%, Ni: 3.06%, Al: 0.030%, Cu: 0.10%, Nb: 0.03%, V: 0.04%, B: 0.0020%, Ca: 0.0025%, P: 0.010%, S: 0.02%, O: 0.0018%, N: 0.0053%, H: 0.00016%, W: 0.013%, and the balance is Fe and unavoidable impurity elements.
[0059] The preparation process of 220mm thick high-strength and tough homogeneous target plate is as follows:
[0060] (1) Hot metal pretreatment: Hot metal is pretreated by KR and deep desulfurization is performed, and the sulfur content is 0.002% at the end of the treatment.
[0061] (2) Smelting. A 100-ton converter is used for smelting, and the molten steel is alloyed when tapping. Then, the LF furnace is refining for 45 minutes. The composition and temperature of the molten steel are adjusted in the LF furnace, and deoxidizer is added for deoxidation. Then, the RH is vacuum degassed, with a vacuum degree of 63Pa and a high vacuum time of 15 minutes to enhance the effect of vacuum degassing and improve the purity of the molten steel.
[0062] (3) Pouring. The die casting process is adopted, and low superheat argon is used to protect the pouring throughout the process. The superheat is controlled at 25-40℃, and the molten steel is cast into a 35-ton flat steel ingot with a thickness of 780mm. After the steel ingot is demolded, it is placed in a slow cooling pit for 48 hours. After the steel ingot is removed from the pit, it is cleaned with warm water at a cleaning temperature of 210℃.
[0063] (4) Heating: The steel ingot is heated in a soaking furnace at a soaking temperature of 1230-1260°C.
[0064] (5) Rolling. A single-stand low-speed large reduction process is adopted, and the rolling speed is controlled at 1.0-1.5 m / s. The single-pass reduction rate is increased as much as possible. The first four passes utilize the high-temperature austenite recrystallization stage of the slab, and the reduction amount of each pass is 45-55 mm. The steel plate is not rolled at warm temperature, and the final rolling temperature is 912°C. The steel plate rolling reduction ratio is ≥3. After rolling, the steel plate is put into the slow cooling pit off the line, the off-line temperature is 490°C, and the slow cooling time is 50h.
[0065] (6) Quenching. The steel plate is heated in a trolley furnace, the quenching heating temperature is 880°C, the holding time is 2.3 min / mm, and after heating and holding, it is quickly hoisted into a water tank, the water cooling time is 130 min, and quenched to room temperature.
[0066] (7) Tempering. The steel plate is tempered by heating in a trolley furnace at a temperature of 650°C-680°C, a holding time of 3.8 min / mm, and then air-cooled to room temperature.
[0067] (8) NDT. The steel plates are tested according to GB / T2970-2016, and the quality grade of the steel plates meets the I grade standard.
[0068] (9) Cutting and printing: According to the order requirements, the steel plate is cut into the required homogeneous target plate size using plasma cutting and printed with markings.
[0069] The properties of the high-strength and tough homogeneous target plate produced using the above process and method are as follows:
[0070] Yield strength is 736MPa, tensile strength is 898MPa, elongation is 18%, and cross-sectional shrinkage is 53%; Charpy impact energy at 20℃ is 117J, and Charpy impact energy at -40℃ is 82J. The fracture test results are fibrous grade 2, slate grade 1, and stratified grade 1. The metallographic structure in the thickness direction of the target plate is uniform tempered troostite.
[0071] Example 3
[0072] The chemical composition of the 120mm thick high-strength and tough homogeneous target plate is: C: 0.31%, Si: 0.26%, Mn: 0.50%, Cr: 2.10%, Mo: 0.35%, Ni: 2.95%, Al: 0.040%, Cu: 0.13%, Nb: 0.04%, V: 0.05%, B: 0.0020%, Ca: 0.0025%, P: 0.010%, S: 0.003%, O: 0.0018%, N: 0.0053%, H: 0.00016%, W: 0.013%, and the balance is Fe and unavoidable impurity elements.
[0073] The preparation process of 120mm thick high-strength and tough homogeneous target plate is as follows:
[0074] (1) Hot metal pretreatment: Hot metal is pretreated by KR and deep desulfurization is performed, and the sulfur content is 0.002% at the end of the treatment.
[0075] (2) Smelting. A 100-ton electric furnace is used for smelting, and the molten steel is alloyed when tapping. Then the LF furnace is refining for 50 minutes, the composition and temperature of the molten steel are adjusted in the LF furnace, and deoxidizer is added for deoxidation. Then it is vacuum degassed in VD, with a vacuum degree of 72Pa and a high vacuum time of 19 minutes. The gas impurities in the molten steel are reduced through the effect of vacuum degassing.
[0076] (3) Pouring. The mold casting process is adopted, and low superheat argon is used to protect the pouring throughout the process. The superheat is controlled at 25-40℃, and the molten steel is cast into a 25-ton flat ingot with a thickness of 600mm. After the ingot is demolded, it is placed in a slow cooling pit for 48 hours. After the ingot is removed from the pit, it is cleaned with warm water at a cleaning temperature of 220℃.
[0077] (4) Heating: The steel ingot is heated in a soaking furnace at a soaking temperature of 1230-1260°C.
[0078] (5) Rolling. A single-stand low-speed high-reduction process is adopted, and the rolling speed is controlled at 1.0-1.5 m / s. The single-pass reduction rate is increased as much as possible, and the reduction amount of each of the first four passes is 40-50 mm. The waiting thickness of the steel plate is 1.8 times the finished product thickness, the starting rolling temperature is 880°C, and the final rolling temperature is 830°C. The steel plate rolling reduction ratio is ≥3, and the steel plate after rolling is put into the slow cooling pit at a temperature of 520°C and a slow cooling time of 49 hours.
[0079] (6) Quenching. The steel plate is heated and quenched in a continuous furnace. The quenching heating temperature is 880°C and the holding time is 2.2 min / mm. After heating and holding, the steel plate is rapidly water-cooled to below the martensitic transformation point in the quenching machine. After exiting the water, the steel plate is returned to a temperature of 60°C and then air-cooled to room temperature.
[0080] (7) Tempering. The steel plate is heated and tempered in a continuous furnace at a temperature of 650°C-680°C, a holding time of 3.5 min / mm, and then air-cooled to room temperature.
[0081] (8) NDT. The steel plates are tested according to GB / T2970-2016, and the quality grade of the steel plates meets the I grade standard.
[0082] (9) Cutting and printing: According to the order requirements, use plasma cutting to cut the steel plate into the homogeneous target plate size required by the order, and print the mark.
[0083] The properties of the high-strength and tough homogeneous target plate produced using the above process and method are as follows:
[0084] Yield strength 799MPa, tensile strength 945MPa, elongation 18%, cross-sectional shrinkage 56%; 20℃ Charpy impact energy 106J, -40℃ Charpy impact energy 78J, fracture test results are fibrous level 1, slate level 1, stratified level 1. The metallographic structure in the thickness direction of the target plate is uniform tempered troostite.
[0085] Example 4
[0086] The preparation process of 100mm thick high-strength and tough homogeneous target plate with normalizing process is as follows:
[0087] (1) Smelting. A 100-ton electric furnace is used for smelting, and the molten steel is alloyed when tapping. The molten steel is then hoisted to the LF furnace for refining for 50 minutes. The composition and temperature of the molten steel are adjusted in the LF furnace, and deoxidizer is added for deoxidation. Next, the molten steel is sent to the VD furnace for vacuum degassing, with a vacuum degree of 63Pa and a high vacuum time of 18 minutes. The vacuum degassing treatment is used to reduce gas impurities in the molten steel.
[0088] (2) Pouring. The mold casting process is adopted, and low superheat argon is used to protect the pouring throughout the process. The superheat is controlled at 25-45℃, and the molten steel is cast into a 30-ton flat steel ingot with a thickness of 700mm. After the steel ingot is demolded or covered, it is slowly cooled for more than 24 hours. After the steel ingot is slowly cooled, it is cleaned with warm water at a temperature of 200℃ to prevent cracks caused by excessive cooling.
[0089] (3) Heating: The steel ingot is heated in a soaking furnace with a soaking temperature of 1230-1260°C.
[0090] (4) Rolling. A single-stand low-speed large reduction process is adopted, and the rolling speed is controlled at 1.0-1.5m / s. The single-pass reduction rate is increased as much as possible. The first four passes utilize the high-temperature austenite recrystallization stage of the slab, and the reduction amount of each pass is 45-55mm. The waiting thickness of the steel plate is 2.0 times the finished product thickness, the starting rolling temperature is 880℃, and the final rolling temperature is 830℃. The rolling reduction ratio of the steel plate is ≥3. After rolling, the steel plate is put into the slow cooling pit for slow cooling, the offline temperature is ≥400℃, and the slow cooling time is ≥48h.
[0091] (5) Normalizing heat treatment. In order to obtain a more uniform structure and better mechanical properties, the steel plate is subjected to normalizing heat treatment before quenching. The normalizing heating temperature is 880-900℃, the holding time is 2.0min / mm, and then air cooling.
[0092] (6) Offline quenching. The quenching heating temperature is 880℃, and the holding time is 2.3min / mm. The steel plate is heated in a trolley furnace and quenched in a water tank. After heating and holding, it is quickly immersed in water. The water cooling time is 130min and quenched to room temperature.
[0093] (7) Tempering. The steel plate is quenched in a trolley furnace with a heating temperature of 650-680°C and a holding time of 3.6 min / mm. After holding, it is air-cooled to room temperature.
[0094] (8) NDT: The steel plates are tested according to GB / T2970-2016 standard, and the quality grade of the steel plates meets the requirements of Grade I.
[0095] (9) Cutting and printing: According to the order requirements, the steel plate is cut into the required homogeneous target plate size using plasma cutting and printed with markings.
[0096] The properties of the high-strength and tough homogeneous target plate produced using the above process and method are as follows:
[0097] Yield strength is 815MPa, tensile strength is 943MPa, elongation is 18%, and cross-sectional shrinkage is 55%; Charpy impact energy at 20℃ is 128J, and Charpy impact energy at -40℃ is 95J. The fracture test results are fibrous level 1, slate level 1, and stratified level 1. The metallographic structure in the thickness direction of the target plate is uniform tempered troostite. The final structure of the steel plate treated with the normalizing process is consistent with that of the directly quenched and tempered steel plate, but the grains are further refined and the mechanical properties are improved.
[0098] Finally, it should be noted that the above embodiments are only used to illustrate rather than limit the technical solutions of the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. Any modification or partial replacement that does not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A 100mm-400mm thick ultra-large specification high-strength and tough homogeneous target plate, characterized by: The chemical composition of the target plate is calculated by mass percentage as follows: C: 0.20-0.35%, Si: 0.15-0.40%, Mn: 0.30-0.70%, Cr: 1.80-2.60%, Mo: 0.28-0.50%, Ni: 2.50-3.50%, Al: 0.015-0.080%, Cu: ≤0.25%, Nb: 0.01-0.05%, V: 0.02-0.08%, B: 0.001-0.005%, Ca: 0.001-0.005%, P: ≤0.012%, S: ≤0.005%, O: ≤0.002%, N: ≤0.008%, H: ≤0.0002%, W: ≤0.13%, and the balance is Fe and unavoidable impurity elements; The target plate has a uniform tempered troostite structure; the yield strength of the target plate is greater than 600 MPa, the tensile strength is greater than 800 MPa, the elongation is greater than or equal to 15%, and the cross-sectional shrinkage is greater than or equal to 50%; the Charpy impact energy at 20°C is greater than or equal to 120 J, and the Charpy impact energy at -40°C is greater than or equal to 70 J; the fracture is inspected according to the GJB 31A-2000 standard, and there are no white spots on the fracture, and the fibrous, slate-like, and stratified grades are 1-2; the steel plate is inspected according to the GB / T2970-2016 standard, and meets the Grade I requirement.
2. A method for producing the 100mm-400mm thick ultra-large specification high-strength and tough homogeneous target plate according to claim 1, characterized in that: include, Step 1, molten steel smelting: smelt molten steel according to the chemical composition of the target plate. In order to ensure the uniformity of the performance of the steel plate target plate, strict requirements are placed on the gas content in the molten steel, O≤13ppm, H≤2.0ppm, N≤50ppm; Step 2: Pouring: Using the die casting process, the molten steel is cast into a flat steel ingot with a thickness of ≥780mm and a single weight of ≥35 tons. After the steel ingot is demoulded, it is slowly cooled for more than 24 hours. After the steel ingot is slowly cooled, it is cleaned with warm water at a cleaning temperature of ≥200℃. Step 3, heating: the steel ingot is heated to 1230-1260℃; Step 4, rolling: adopt low-speed large reduction process, the rolling speed is controlled at 1.0-1.5m / s, the first 4 passes use the high-temperature austenite recrystallization stage of the slab, set the reduction of each pass to 40-60mm, for the production thickness>200mm steel plate, no warm rolling, that is, no controlled rolling, directly rolled to the final plate thickness, the final rolling temperature ≥900℃; for the production thickness ≤200mm steel plate, the warm thickness is 1.5-2.0 times the finished product thickness, the steel plate rolling reduction ratio is ≥5, the starting rolling temperature is 850-900℃, and the final rolling temperature is 800-850℃; after rolling, the steel plate is slowly cooled off the line, the off-line temperature is ≥400℃, and the slow cooling time is ≥48h; Step 5, offline quenching: quenching heating temperature 860-900℃, holding time 2.0-2.5min / mm, steel plates with a thickness of less than 150mm are heated and held, and then quickly water-cooled to below the martensitic phase transformation point, and the steel plate leaving water temperature is controlled to be 50-70℃, and then the target temperature is returned to 50-80℃, and then air-cooled to room temperature; steel plates with a thickness greater than 150mm are heated and held, and then quickly put into water, and the water cooling time is 120-150min, and quenched to room temperature; Step 6. Tempering: heating temperature 650℃-680℃, holding time 3.5-4min / mm*steel plate thickness mm, cool to room temperature after holding.
3. The method for producing a 100mm-400mm thick ultra-large specification high-strength and tough homogeneous target plate according to claim 2, characterized in that: Step 1, molten steel smelting includes KR molten iron pretreatment, primary refining, LF refining, and vacuum degassing, wherein S≤0.003% after KR molten iron pretreatment, and the alloy content in the molten steel is adjusted and deoxidized during the LF refining process. The high vacuum time in the vacuum degassing stage is ≥15min, and the vacuum degree of the vacuum chamber is set to <133Pa.
4. The method for producing a 100mm-400mm thick ultra-large specification high-strength and tough homogeneous target plate according to claim 2, characterized in that: Step 2: Use low superheat argon to protect the pouring during the entire casting process, control the superheat at 25-45°C, and place the steel ingot into a slow cooling pit or add a cover for slow cooling.
5. The method for producing a 100mm-400mm thick ultra-large specification high-strength and tough homogeneous target plate according to claim 2, characterized in that: Step 5: The quenching and heating of steel plates with a thickness of less than 150 mm are carried out in a continuous furnace. After heating and insulation, they are quickly water-cooled in a quenching machine; steel plates with a thickness of more than 150 mm are heated in a trolley furnace and quenched in a water tank.
6. The method for producing a 100mm-400mm thick ultra-large specification high-strength and tough homogeneous target plate according to claim 2, characterized in that: Step six, the tempering heating of steel plates with a thickness of less than 150 mm is carried out in a continuous furnace, and the tempering of steel plates with a thickness of more than 150 mm is carried out in a trolley furnace.
7. The method for producing a 100mm-400mm thick ultra-large specification high-strength and tough homogeneous target plate according to claim 2, characterized in that: In order to reduce the segregation in the structure, the steel plate is normalized before the quenching treatment in step 5. The normalizing heating temperature is 880-900°C, the holding time is 1.8-2.5min / mm, and then air-cooled.
8. The method for producing a 100mm-400mm thick ultra-large specification high-strength and tough homogeneous target plate according to claim 2, characterized in that: In order to improve the quality of flaw detection on the surface and core of the steel plate, the steel ingot is opened before the rolling step, and the reduction rate of the opening is 50%-60%.