A sodium ion battery negative electrode material and preparation method thereof
By preparing active materials with loose graphene clusters supporting bismuth oxide, the problem of pulverization caused by volume expansion during sodium ion insertion and extraction in sodium-ion battery anode materials was solved, and a sodium-ion battery anode material with high specific capacity and good stability was achieved.
Patent Information
- Application Number
- CN202310165681.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-02-27
AI Technical Summary
The pulverization of sodium-ion battery anode materials due to volume expansion during sodium ion insertion and extraction affects battery stability.
The sodium-ion battery anode material is composed of glassy carbon sheets and an active layer. The active layer consists of loaded active materials, conductive agents, and binders. Loose graphene clusters loaded with bismuth oxide are prepared by a specific method to form a flower-like cluster structure, which enhances the loading performance and stability.
It improves the specific capacity and charge-discharge stability of sodium-ion batteries, with an initial reversible specific capacity of 165.2-173.9 mAh·g⁻¹ and a capacity retention of 81.66-88.26% after 500 cycles, significantly enhancing the stability of the anode material.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery materials, and in particular, relates to a sodium ion battery negative electrode material and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have been favored by the market since their advent and are the main commercial energy storage devices today. However, with the gradual increase in demand for rechargeable batteries, the problem of lithium resource scarcity has gradually emerged. For large-scale energy storage devices, the high price of lithium has greatly limited the scale of application.
[0003] Sodium and lithium have similar equilibrium potentials and physical and chemical properties, and are abundant in the earth's crust, with an abundance of 2.75%. Sodium is an ideal substitute for lithium. Therefore, it was developed in the 1980s. It is similar to lithium-ion batteries in principle: during the charge and discharge process, Na + The Na + It is deintercalated from the positive electrode and embedded in the negative electrode through the electrolyte, and the opposite is true during discharge; structurally: it includes positive electrode material, separator, negative electrode material and electrolyte; among them, the negative electrode material is an important component of the sodium ion battery, which plays the role of sodium ion storage and release during the cycle process. However, sodium ions have a large ionic radius, and a violent volume expansion will occur during the process of sodium ions embedding into the negative electrode material, and the opposite is true during deintercalation, thereby causing the negative electrode material to pulverize, and thus making the stability of the sodium ion battery poor. The present invention starts from improving the stability of the sodium ion battery and develops a negative electrode material for a sodium ion battery. Summary of the invention
[0004] In order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide a sodium ion battery negative electrode material and a preparation method thereof.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] A sodium ion battery negative electrode material consists of a glassy carbon sheet and an active layer, wherein the active layer comprises, by weight, 75-82 parts of a loaded active material, 10-14 parts of a conductive agent and 8-12 parts of a binder.
[0007] The loaded active material was prepared by the following method:
[0008] Step A1: Diethylenetriamine and deionized water are mixed evenly, nitrogen is introduced for protection, the temperature is raised to 45-55°C, graphene oxide is slowly added under ultrasonic dispersion, and then the temperature is raised to 90-95°C for reflux reaction for 3-4 hours, diethylenetriamine reacts with oxygen-containing groups on the surface of graphene oxide, and under the effect of steric hindrance, the thin flake graphene oxide sheets present irregular wrinkles, after the reaction, the precipitate is centrifuged and dried to break up, and then placed in an oxidation furnace for calcination at 220-260°C for 2-2.5 hours to shape, so as to prepare wrinkled graphene;
[0009] Furthermore, the usage ratio of graphene oxide, diethylenetriamine and deionized water is 10 g: 1.6-1.9 mL: 65-75 mL.
[0010] Step A2: stirring and dissolving branched polyethyleneimine, tetrahydrofuran and ethanol under nitrogen protection, placing in an ice-water bath to maintain constant temperature, slowly adding di-tert-butyl dicarbonate dilution dropwise under ultrasonic dispersion to react for 1.5-2h, wherein a small amount of di-tert-butyl dicarbonate reacts with part of the amino groups in the branched polyethyleneimine to protect part of the amino groups, thereby preparing an assembly solution;
[0011] Furthermore, the usage ratio of branched polyethyleneimine, di-tert-butyl dicarbonate, tetrahydrofuran and ethanol is 10 mL: 8-11 mmol: 140-170 mL: 5-7 mL, and the concentration of the di-tert-butyl dicarbonate diluent is 10%.
[0012] Step A3: Two-thirds of the amount of wrinkled graphene and the assembly solution are mixed, and after applying 20kHz ultrasonic dispersion, the mixture is placed in a water bath and reacted at a constant temperature of 35-42°C for 40-50min, and then trifluoroacetic acid is added dropwise and stirred for 1-1.2h to deprotect the protected amino group, and then triethylamine is added for neutralization, and the remaining amount of wrinkled graphene is slowly added, and stirred at 150-200rpm for 12h. The wrinkled graphene is slowly assembled with branched polyethyleneimine as the core to form a cluster structure. After the reaction, the precipitate is centrifuged and placed in a hydrazine hydrate solution for immersion for 24h, and the precipitate is centrifuged again and washed and dried with an ethanol solution to prepare a loose graphene cluster;
[0013] Furthermore, the usage ratio of the wrinkled graphene, the assembly solution and the trifluoroacetic acid is 10 g: 120-150 mL: 1.4-1.7 mL.
[0014] Step A4: Stir and dissolve bismuth nitrate and acetone, add loose graphene clusters and stir and mix at high speed, heat to 50-58° C. and reflux, slowly add sodium carbonate solution until the pH value is 8.0-8.5, keep warm and stand for conversion for 1.4-1.6 hours, bismuth nitrate reacts with sodium carbonate to generate bismuth carbonate which is deposited in the surface pores of the loose graphene clusters, centrifuge to take out the filter cake, rinse and dry it, then place it in a vacuum furnace, roast it at 310-320° C. for 1.8-2.2 hours, and break it up after cooling to prepare a loaded active material;
[0015] Furthermore, the usage ratio of the loose graphene clusters, bismuth nitrate and acetone is 10 g: 2.2-2.5 g: 80-100 mL.
[0016] A method for preparing a negative electrode material for a sodium ion battery comprises the following steps:
[0017] Step S1: uniformly mix the loaded active material, the conductive agent and the binder, add a solvent, stir and mix to form a negative electrode slurry;
[0018] Step S2: After cleaning the surface of the glassy carbon sheet, the negative electrode slurry is scraped and applied, and the sheet is placed in a vacuum drying oven for drying to form an active layer, thereby preparing a negative electrode material for a sodium ion battery.
[0019] Preferably, the conductive agent is acetylene black, the adhesive is polyvinylidene fluoride, and the solvent is N-methyl-2-pyrrolidone.
[0020] Beneficial effects of the present invention:
[0021] The invention prepares an active material of loose graphene clusters loaded with bismuth oxide, and applies the loose graphene clusters in a sodium ion battery to obtain good stability; wherein the loose graphene clusters are modified by diethylenetriamine on graphene oxide, and the loose graphene clusters are used to react with oxygen-containing groups on the surface of the graphene oxide, so that the graphene presents a wrinkled sheet structure, and branched polyethyleneimine is used as an assembly template, and a small amount of di-tert-butyl dicarbonate is used to shield part of the amino groups of the branched polyethyleneimine, and assembly is performed in batches to avoid too fast assembly of the graphene, resulting in uneven structure, thereby forming load performance and stability, and the obtained loose graphene clusters present a flower-like cluster structure, have a large active loading surface, improve the loadability and loading amount of bismuth compounds, and have a certain improvement on the specific capacity of the battery. After testing, 0.5A·g -1 At the current density, the first reversible specific capacity reached 165.2-173.9 mAh g -1 Compared with the existing bismuth / carbon-based sodium-ion batteries, the specific capacity is significantly improved; the wrinkled graphene clusters have good toughness and can maintain a good shape during the embedding and de-embedding of sodium ions, effectively reducing the pulverization of the negative electrode material and greatly improving the charge and discharge stability of the negative electrode material. After testing, at 20A·g -1 After 500 cycles at high current density, the capacity retention rate is still 81.66-88.26%, which is significantly improved compared with existing bismuth / carbon-based sodium ion batteries. Implementation
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example
[0023] The present invention prepares the negative electrode material of the sodium ion battery, and the specific implementation process is as follows:
[0024] 1. Preparation of loaded active materials
[0025] a1. Take diethylenetriamine and deionized water and stir and mix them evenly, introduce nitrogen to expel the air, heat the water bath to 55°C, apply 33kHz ultrasonic dispersion, slowly and uniformly add graphene oxide within 10 minutes, then stop ultrasonic dispersion, apply 200rpm stirring and heat to 95°C for reflux reaction for 3 hours. In the above reaction, the amount ratio of graphene oxide, diethylenetriamine and deionized water is 10g:1.9mL:75mL. After the reaction, centrifuge to obtain the precipitate, dry it at 80°C for 3 hours, and then place it in an oxidation furnace with air atmosphere, heat it to 260°C and roast it for 2 hours to fix it, and obtain wrinkled graphene.
[0026] a2. Take a reactor and pass nitrogen into the reactor for protection. Add branched polyethyleneimine (the nominal average molecular weight is 600, the same below), tetrahydrofuran and ethanol and stir to mix evenly. Place it in an ice water bath to maintain constant temperature. Take a tetrahydrofuran dilution of di-tert-butyl dicarbonate and adjust the concentration to 10%. Under 28kHz ultrasonic dispersion, add the dilution of di-tert-butyl dicarbonate to react within 1.5 hours. In the above reaction, the amount ratio of branched polyethyleneimine, di-tert-butyl dicarbonate, tetrahydrofuran and ethanol is 10mL:11mmol:170mL:7mL, and the assembly solution is obtained.
[0027] a3. Take the wrinkled graphene and distribute it in a weight ratio of 2:1. First, add 2 / 3 of the wrinkled graphene to the assembly solution, disperse it ultrasonically at 20kHz, and heat the dispersion in a water bath at the same time. React at 42°C for 40 minutes, then drop trifluoroacetic acid, stir at 150rpm for 1h, neutralize it with triethylamine, and then stir at 200rpm. Slowly add the remaining wrinkled graphene within 6h, and continue to react after adding. Control the overall reaction time to be 12h. In the above reaction, the total amount of wrinkled graphene, assembly solution and trifluoroacetic acid are used in a ratio of 10g:150mL:1.7mL. After the reaction, centrifuge to obtain the precipitate, place it in a 30% hydrazine hydrate solution and soak it for 24h. Centrifuge again to obtain the precipitate, wash it with ethanol solution and dry it to obtain loose graphene clusters.
[0028] a4. Take bismuth nitrate and acetone and stir to dissolve, add loose graphene clusters and stir at 800 rpm for 10 minutes, heat to 58°C and reflux, slowly add 0.2 mol / L sodium carbonate solution until the pH value reaches 8.5, keep warm and stand for conversion for 1.4 hours. In the above reaction, the amount ratio of loose graphene clusters, bismuth nitrate and acetone is 10g:2.5g:100mL. After the reaction, centrifuge to take the filter cake for elution, dry it at 60°C for 2 hours under nitrogen atmosphere, then place it in a vacuum furnace, roast it at 320°C for 1.8 hours, and break it up into a uniform powder at high speed after cooling to obtain a loaded active material.
[0029] 2. Preparation of negative electrode materials
[0030] s1. Take 75 parts of the above-prepared loaded active material, 11 parts of the conductive agent acetylene black and 8 parts of the binder polyvinylidene fluoride according to the weight ratio, stir and mix evenly, slowly add the solvent N-methyl-2-pyrrolidone under stirring at 240 rpm, and adjust the viscosity to 6000 mPa·s for uniform coating to obtain a negative electrode slurry;
[0031] s2. Take a glassy carbon sheet, wipe it with anhydrous ethanol, dry it with hot air, clean the glassy carbon sheet, then scrape and apply the negative electrode slurry on the cleaned surface of the glassy carbon sheet, place it in a vacuum drying oven, and dry it at 85°C for 6 hours to obtain the negative electrode material for the sodium ion battery. Example
[0032] The present invention prepares the negative electrode material of the sodium ion battery, and the specific implementation process is as follows:
[0033] 1. Preparation of loaded active materials
[0034] a1. Take diethylenetriamine and deionized water and stir and mix them evenly, introduce nitrogen to expel the air, heat the water bath to 45°C, apply 33kHz ultrasonic dispersion, slowly and uniformly add graphene oxide within 10 minutes, then stop ultrasonic dispersion, apply 200rpm stirring and heat to 90°C for reflux reaction for 4 hours. In the above reaction, the amount ratio of graphene oxide, diethylenetriamine and deionized water is 10g:1.6mL:65mL. After the reaction, centrifuge to obtain the precipitate, dry it at 80°C for 3 hours, and then place it in an oxidation furnace with air atmosphere, heat it to 220°C and roast it for 2.5 hours to fix it, and obtain wrinkled graphene.
[0035] a2. Take a reactor and pass nitrogen into it for protection. Add branched polyethyleneimine, tetrahydrofuran and ethanol and stir to mix evenly. Place it in an ice water bath to maintain constant temperature. Take a dilution of di-tert-butyl dicarbonate in tetrahydrofuran and adjust the concentration to 10%. Under 28kHz ultrasonic dispersion, add the dilution of di-tert-butyl dicarbonate to react within 2 hours. In the above reaction, the amount ratio of branched polyethyleneimine, di-tert-butyl dicarbonate, tetrahydrofuran and ethanol is 10mL:8mmol:140mL:5mL, and the assembly solution is obtained.
[0036] a3. Take the wrinkled graphene and distribute it in a weight ratio of 2:1. First, add 2 / 3 of the wrinkled graphene to the assembly solution, disperse it ultrasonically at 20kHz, and heat the dispersion in a water bath at the same time. React at 35°C for 50 minutes, then add trifluoroacetic acid dropwise, stir at 150rpm for 1.2h, neutralize it with triethylamine, and stir at 150rpm again. Slowly add the remaining wrinkled graphene within 8h, and continue to react after adding. Control the overall reaction time to be 12h. In the above reaction, the total amount of wrinkled graphene, assembly solution and trifluoroacetic acid are used in a ratio of 10g:120mL:1.4mL. After the reaction, centrifuge to obtain the precipitate, place it in a 30% hydrazine hydrate solution and soak it for 24h. Centrifuge again to obtain the precipitate, wash it with ethanol solution and dry it to obtain loose graphene clusters.
[0037] a4. Stir and dissolve bismuth nitrate and acetone, add loose graphene clusters and stir at 800 rpm for 10 min, heat to 50°C and reflux, slowly add 0.2 mol / L sodium carbonate solution until the pH value reaches 8.0, keep warm and let stand for conversion for 1.6 h. In the above reaction, the amount ratio of loose graphene clusters, bismuth nitrate and acetone is 10 g: 2.2 g: 80 mL. After the reaction, centrifuge to take the filter cake for elution, dry it at 60°C for 2 h under nitrogen atmosphere, then place it in a vacuum furnace, roast it at 310°C for 2.2 h, and break it up into a uniform powder at high speed after cooling to obtain a loaded active material.
[0038] 2. Preparation of negative electrode materials
[0039] s1. Take 82 parts of the above-prepared loaded active material, 14 parts of the conductive agent acetylene black and 12 parts of the binder polyvinylidene fluoride according to the weight ratio, stir and mix evenly, slowly add the solvent N-methyl-2-pyrrolidone under stirring at 240 rpm, and adjust the viscosity to 6000 mPa·s for uniform coating to obtain a negative electrode slurry;
[0040] s2. Take a glassy carbon sheet, wipe it with anhydrous ethanol, dry it with hot air, clean the glassy carbon sheet, then scrape and apply the negative electrode slurry on the cleaned surface of the glassy carbon sheet, place it in a vacuum drying oven, and dry it at 85°C for 6 hours to obtain the negative electrode material for the sodium ion battery. Example
[0041] The present invention prepares the negative electrode material of the sodium ion battery, and the specific implementation process is as follows:
[0042] 1. Preparation of loaded active materials
[0043] a1. Take diethylenetriamine and deionized water and stir to mix evenly, introduce nitrogen to expel air, heat the water bath to 52°C, apply 33kHz ultrasonic dispersion, slowly and uniformly add graphene oxide within 10 minutes, then stop ultrasonic dispersion, apply 200rpm stirring and heat to 95°C for reflux reaction for 3.2 hours. In the above reaction, the amount ratio of graphene oxide, diethylenetriamine and deionized water is 10g:1.8mL:75mL. After the reaction, centrifuge to obtain the precipitate, dry it at 80°C for 3 hours, and then place it in an oxidation furnace with air atmosphere, heat it to 240°C and roast it for 2.3 hours to fix it, and obtain wrinkled graphene.
[0044] a2. Take a reactor and pass nitrogen into the reactor for protection. Add branched polyethyleneimine, tetrahydrofuran and ethanol and stir to mix evenly. Place it in an ice water bath to maintain constant temperature. Take a dilution of di-tert-butyl dicarbonate in tetrahydrofuran and adjust the concentration to 10%. Under 28kHz ultrasonic dispersion, add the dilution of di-tert-butyl dicarbonate within 1.8 hours to react. In the above reaction, the amount ratio of branched polyethyleneimine, di-tert-butyl dicarbonate, tetrahydrofuran and ethanol is 10mL:10mmol:160mL:6mL, and the assembly solution is obtained.
[0045] a3. Take the wrinkled graphene and distribute it in a weight ratio of 2:1. First, add 2 / 3 of the wrinkled graphene to the assembly solution, disperse it ultrasonically at 20kHz, and heat the dispersion in a water bath at the same time. React at 38°C for 45 minutes, then add trifluoroacetic acid dropwise, stir at 150rpm for 1.2h, neutralize it with triethylamine, and then stir at 200rpm. Slowly add the remaining wrinkled graphene within 6.5h, and continue to react after adding. Control the overall reaction time to be 12h. In the above reaction, the total amount of wrinkled graphene, assembly solution and trifluoroacetic acid are used in a ratio of 10g:130mL:1.6mL. After the reaction, centrifuge to obtain the precipitate, place it in a 30% hydrazine hydrate solution and soak it for 24h. Centrifuge again to obtain the precipitate, wash it with ethanol solution and dry it to obtain loose graphene clusters.
[0046] a4. Take bismuth nitrate and acetone and stir to dissolve, add loose graphene clusters and stir at 800 rpm for 10 minutes, heat to 55°C and reflux, slowly add 0.2 mol / L sodium carbonate solution until the pH value reaches 8.0, keep warm and stand for conversion for 1.5 hours. In the above reaction, the amount ratio of loose graphene clusters, bismuth nitrate and acetone is 10g:2.4g:90mL. After the reaction, centrifuge to take the filter cake for elution, dry it at 60°C for 2 hours under nitrogen atmosphere, then place it in a vacuum furnace, roast it at 310°C for 2 hours, and break it up into a uniform powder at high speed after cooling to obtain a loaded active material.
[0047] 2. Preparation of negative electrode materials
[0048] s1. Take 78 parts of the above-prepared loaded active material, 10 parts of the conductive agent acetylene black and 10 parts of the binder polyvinylidene fluoride according to the weight ratio, stir and mix evenly, slowly add the solvent N-methyl-2-pyrrolidone under stirring at 240 rpm, and adjust the viscosity to 6000 mPa·s for uniform coating to obtain a negative electrode slurry;
[0049] s2. Take a glassy carbon sheet, wipe it with anhydrous ethanol, dry it with hot air, clean the glassy carbon sheet, then scrape and apply the negative electrode slurry on the cleaned surface of the glassy carbon sheet, place it in a vacuum drying oven, and dry it at 85°C for 6 hours to obtain the negative electrode material for the sodium ion battery.
[0050] The negative electrode material prepared above was cut into a disc with a diameter of 16 mm as the negative electrode, an olivine NaFePO4 positive electrode, a Whatman glass fiber filter membrane as the diaphragm, and an electrolyte of NaPF6. A CR2032 battery was formed in an argon atmosphere. The charge and discharge test was carried out using a blue electric test system, and the test current density was 0.5 A g -1 , 2A·g -1 , and 20A·g -1 , respectively detect the first reversible specific capacity and the number of cycles is 500 times, the specific test data are shown in Table 1:
[0051] Table 1
[0052]
[0053] From the data in Table 1, it can be seen that the negative electrode material prepared by the present invention is used in sodium ion batteries, 0.5A·g -1 At the current density, the first reversible specific capacity reached 165.2-173.9 mAh g -1 , 2A·g -1 At the current density, the first reversible specific capacity reached 151.8-156.7 mAh g -1 , 20A·g -1At the current density, the first reversible specific capacity reached 105.7-114.2 mAh g -1 , showing high specific capacity; after 500 cycles test, 0.5A·g -1 Under current density, the capacity retention rate is 96.26-97.90%, at 20A·g -1 Under high current density, the capacity retention rate is still 81.66-88.26%, showing excellent stability.
[0054] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0055] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A negative electrode material for a sodium ion battery, comprising a glassy carbon sheet and an active layer, characterized in that: The active layer comprises, by weight: 75-82 parts of loaded active material, 10-14 parts of conductive agent and 8-12 parts of adhesive; The loaded active material is prepared by the following method: Step A1: diethylenetriamine and deionized water are mixed, the temperature is raised to 45-55°C under nitrogen protection, graphene oxide is slowly added under ultrasonic dispersion, and then the temperature is raised to 90-95°C for reflux reaction for 3-4 hours. After the reaction, the precipitate is centrifuged and dried and dispersed, and then placed in an oxidation furnace for calcination at 220-260°C for 2-2.5 hours to shape, thereby preparing wrinkled graphene; Step A2: stirring and dissolving branched polyethyleneimine, tetrahydrofuran and ethanol under nitrogen protection, placing in an ice-water bath to maintain constant temperature, slowly adding di-tert-butyl dicarbonate dilution dropwise under ultrasonic dispersion to react for 1.5-2h to prepare an assembly solution; Step A3: Two-thirds of the wrinkled graphene and the assembly solution are mixed, and after applying 20kHz ultrasonic dispersion, the mixture is placed in a water bath and reacted at a constant temperature of 35-42°C for 40-50 minutes. Trifluoroacetic acid is then added dropwise and stirred for 1-1.2 hours. Triethylamine is then added for neutralization, and the remaining wrinkled graphene is slowly added and stirred for 12 hours. After the reaction, the precipitate is centrifuged and immersed in a hydrazine hydrate solution for 24 hours. The precipitate is centrifuged again and washed and dried with an ethanol solution to prepare loose graphene clusters. Step A4: Stir and dissolve bismuth nitrate and acetone, add loose graphene clusters and stir at high speed, heat to 50-58°C and reflux, slowly add sodium carbonate solution until the pH value is 8.0-8.5, keep warm and stand for conversion for 1.4-1.6 hours, centrifuge to take the filter cake, rinse and dry, then place in a vacuum furnace, roast at 310-320°C for 1.8-2.2 hours, and break up after cooling to make a loaded active material.
2. A sodium ion battery negative electrode material according to claim 1, characterized in that: The usage ratio of graphene oxide, diethylenetriamine and deionized water is 10g:1.6-1.9mL:65-75mL.
3. A sodium ion battery negative electrode material according to claim 2, characterized in that: The usage ratio of branched polyethyleneimine, di-tert-butyl dicarbonate, tetrahydrofuran and ethanol is 10 mL: 8-11 mmol: 140-170 mL: 5-7 mL.
4. A sodium ion battery negative electrode material according to claim 3, characterized in that: The usage ratio of wrinkled graphene, assembly solution and trifluoroacetic acid is 10 g: 120-150 mL: 1.4-1.7 mL.
5. A sodium ion battery negative electrode material according to claim 4, characterized in that: The usage ratio of loose graphene clusters, bismuth nitrate and acetone is 10g:2.2-2.5g:80-100mL.
6. The method for preparing a negative electrode material for a sodium ion battery according to claim 5, characterized in that: The steps include: Step S1: uniformly mix the loaded active material, the conductive agent and the binder, add a solvent, stir and mix to form a negative electrode slurry; Step S2: After cleaning the surface of the glassy carbon sheet, the negative electrode slurry is scraped and applied, and the sheet is placed in a vacuum drying oven for drying to form an active layer, thereby preparing a negative electrode material for a sodium ion battery.
7. The method for preparing a negative electrode material for a sodium ion battery according to claim 6, characterized in that: The conductive agent is acetylene black, the adhesive is polyvinylidene fluoride, and the solvent is N-methyl-2-pyrrolidone.