Preparation method and application of metal powder for workpiece coating

By combining heat treatment of metal powder and laser cladding technology, carbide precipitation is delayed and carbide is precipitated at a specific temperature, solving the problem of low hardness of hard wear-resistant coatings in the prior art, significantly improving the surface of the workpiece The hardness and service life of the coating.

CN116213719BActive Publication Date: 2024-11-26CHINA MASCH INST OF ADVANCED MATERIALS (ZHENGZHOU) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310408050.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-11-26
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

In the prior art, rapid cooling of metal powder during preparation leads to tissue imbalance, and the alloy phase cannot be completely precipitated in the matrix, resulting in low hardness of the hard wear-resistant coating. Laser cladding technology also has similar process characteristics, making it difficult to be significant. Improve coating hardness.

Method used

By heat-treating the metal powder containing carbide-forming elements in an isolated environment of 500-950°C, a phase-change powder is formed to delay the precipitation of carbides, and the carbides are precipitated at a specific temperature in combination with laser cladding technology, which significantly improves melting The hardness of the cladding.

Benefits of technology

It significantly improves the hardness and service life of the wear-resistant coating on the surface of the workpiece, ensures the flowability and tissue phase change of the metal powder, avoids high-temperature melting and adhesion and cracking, and meets the performance requirements of additive manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116213719B_ABST
    Figure CN116213719B_ABST
Patent Text Reader

Abstract

The present invention provides a preparation method and application of metal powder for workpiece coating, which belongs to the field of powder metallurgy and additive manufacturing technology. The present invention phase-changes the metal powder through reasonable heat treatment, and uses the phase-changed metal powder as raw material for additive manufacturing applications, such as laser cladding, to provide a method for high-performance additive manufacturing of coatings or parts. Compared with the existing technical process, this method does not require the addition of additional ceramic hard phases, such as carbides or oxides, and can perform low-temperature heat treatment or additive manufacturing of parts without overall heat treatment and obtain high hardness and good wear resistance, thereby improving the service life of the entire part.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of powder metallurgy and additive manufacturing, and in particular to a preparation method and application of metal powder for workpiece coating. Background Art

[0002] Friction and wear are the most common failure forms of mechanical equipment and its parts, especially in the metallurgical mining, petrochemical and aerospace industries. Therefore, the application of hard wear-resistant coatings has become an effective way to increase the service life of mechanical equipment and its parts, such as shaft parts. During the operation of mechanical equipment, hard wear-resistant coatings will be worn out first and then protect parts from failure, thereby increasing the average trouble-free working time of mechanical equipment and improving its reliability.

[0003] Laser cladding technology can be used for surface modification of metal parts. The laser instantly melts the metal powder at high temperature and then quickly cools it to produce a hard and wear-resistant coating on the surface of the metal parts. The principle is to melt the metal powder onto the metal substrate or workpiece to form a cladding layer. The bonding mode between the cladding layer and the workpiece or metal substrate is a high-strength metallurgical bond. The chemical composition and phase composition of the metal powder are one of the important factors affecting the performance of the hard and wear-resistant coating.

[0004] Among them, the phase composition of the metal powder is formed during the preparation process of the metal powder. The common metal powder preparation method in the prior art is obtained by rapidly solidifying dispersed droplets with a cooling medium. Therefore, the metal powder structure is a rapid cooling structure rather than an equilibrium structure. Some alloy phases cannot precipitate in the matrix, resulting in low hardness of the metal powder. Laser cladding technology also has similar process characteristics, that is, the metal powder is melted in a short time and clad on the workpiece or substrate. Therefore, some alloy phases cannot precipitate in the matrix, and the hardness of the hard wear-resistant coating is low. Patent CN115673314A discloses a method for increasing the hardness of the coating by mixed cladding of metal powder and exogenous carbide. Using laser cladding technology, the metal powder is combined with the exogenous carbide to form MC-type carbide, but the amount of alloy phase precipitated in the matrix is ​​small, which leads to low hardness of the hard wear-resistant coating.

[0005] In the prior art, the hardness of the hard wear-resistant coating is improved by changing the composition and the proportion of each component in the metal powder. Patent CN113265656A discloses a method for obtaining a high-hardness coating using rare earth oxide CeO2 and T15 high-speed steel powder by laser cladding technology. Adding rare earth oxide CeO2 as an exogenous carbide will increase the crack sensitivity of the cladding layer, and the purpose of improving the performance of the hard wear-resistant coating is achieved by controlling the phase composition and its content; however, the hardness of the obtained high-hardness cladding coating is not significantly improved compared to the metal powder before cladding. Summary of the invention

[0006] In view of this, the present invention provides a method for preparing metal powder for workpiece coating and application. Through reasonable heat treatment, carbides are precipitated from the metal powder during the additive manufacturing process, the hardness of the cladding layer is increased, and the service life of the wear-resistant coating on the workpiece surface is greatly improved.

[0007] In order to solve the above technical problems, the present invention provides a method for preparing metal powder for workpiece coating, comprising the following steps:

[0008] The metal powder containing carbide-forming elements is placed in a high-temperature resistant can in an isolated environment, and the metal powder containing carbide-forming elements is heat-treated at 500-950° C. for 12-108 hours; the metal powder is taken out and cooled to room temperature to obtain phase change metal powder.

[0009] The present invention heat treats metal powder containing carbide-forming elements so that carbides in the metal powder cannot be completely precipitated in a short time under the action of a cooling medium in the metal powder preparation process, thereby forming a metal powder in a state to be excited, which can effectively precipitate at a suitable heat treatment temperature and time, thereby increasing the hardness of the cladding layer.

[0010] In this step, the metal powder is screened according to the particle size required by the additive manufacturing process, and the metal powder of the specified particle size is placed in a package. The package can be protected by an argon atmosphere or a vacuum package. The package material can be stainless steel, titanium alloy, corundum, etc.

[0011] The heat treatment holding temperature and time are related to the alloy composition, and the determination of the holding time is also related to the powder particle size. In the practice of holding temperature, when the heat treatment temperature exceeds 950°C, the metal powder will show significant sintering phenomenon, that is, the metal powder loses fluidity and is no longer suitable for additive manufacturing powder raw materials. When the heat treatment temperature is below 500°C, the phase change of the structure is slow, which has no practical operational significance and is not conducive to energy saving and environmental protection.

[0012] In the practice regarding the holding time, after the holding time exceeds 108 hours, the hardness change of the metal powder is no longer significant, that is, the powder phase change process enters a stage with relatively less change. Continuing to increase the holding time has no practical significance and is not conducive to energy conservation and environmental protection. When the holding time is less than 4 hours, the metal powder tissue phase change is slow and has no practical significance.

[0013] Furthermore, the heating rate of the metal powder containing carbide-forming elements during heat treatment is not higher than 10° C. / min.

[0014] Furthermore, the isolated environment is a protective atmosphere or a vacuum environment.

[0015] In order to prevent the loss of sealing of the package at high temperature during the insulation stage, which may lead to high-temperature oxidation of the metal powder, the heat treatment furnace or induction heating equipment is preferably protected by argon atmosphere.

[0016] Furthermore, the chemical formula of the carbide-forming element is MC, M2C, M6C, M7C3 or M 23 C6.

[0017] Furthermore, in the general chemical formula, M is one or more of V, W, Cr, Mo, Ti, Nb, and Hf.

[0018] Another object of the present invention is to provide a method for coating a workpiece using phase change metal powder, comprising the following steps:

[0019] S1. Surface treatment is performed on the parts to be clad, and preheating is performed in the temperature range of 250-350℃;

[0020] S2, cladding the phase change metal powder on the surface treated workpiece to be clad by laser, wherein the process parameters of the laser cladding are: 1500-3000W, laser radius of 0.5-1.5mm, scanning speed of 5-50mm / s, overlap rate of 20-80%, powder feeding rate of 2-50r / min, and argon flow rate of 3-15L / min;

[0021] S3, tempering the cladding part at a temperature range of 520-560° C. for 1-3 times to obtain an additively manufactured workpiece.

[0022] Furthermore, the phase content of the cladding layer changes, and the change in phase content is manifested as an increase in carbide precipitation.

[0023] Furthermore, the hardness of the cladding layer is 55-65hrc.

[0024] Furthermore, the fluidity of the phase change metal powder subjected to laser cladding is 20 to 45 s / 50 g.

[0025] The metal powder prepared by the above method can be applied to additive manufacturing.

[0026] The metal powder after phase change needs to meet certain properties. The metal powder after phase change is subjected to flowability test, X-ray diffraction test, scanning electron microscope observation and metal powder hardness test. The test results are used to determine whether the metal powder meets the additive manufacturing organization and performance requirements.

[0027] The cross section of the cladding part was sampled and, after metallographic sample preparation, the structure was analyzed by optical microscope and scanning electron microscope, and the Vickers microhardness test was performed.

[0028] In summary, compared with the prior art, the present application has at least one of the following beneficial technical effects:

[0029] 1. After adopting the above technical solution, the present invention adds carbide-forming elements to the metal powder, then phase-changes the metal particles, and strictly controls the phase change temperature and time, so that the carbide-forming elements in the metal particle mixture cannot precipitate carbides at a specific temperature. When the obtained phase change metal powder is used in the field of additive manufacturing, it can precipitate granular carbide phases at a specific temperature, and its microstructure enhances the hardness of the metal particles, thereby ensuring that the hardness of the cladding coating is significantly improved. Compared with the existing technology of not performing heat treatment but only changing the composition, it can no longer achieve a significant improvement. The present application can significantly increase the hardness of the cladding layer and increase the service life of the workpiece.

[0030] 2. After adopting the above technical solution, the present invention strictly controls the phase change temperature and time to ensure that the metal particles will not stick together due to high temperature melting, affecting the fluidity of the metal powder, and ensuring that the metal particles do not stick together, so that the metal particles can be successfully used for cladding.

[0031] 3. The present invention also manufactures coatings or components by using appropriate additive manufacturing process parameters, and finally, additively manufactures components by low temperature heat treatment or without overall heat treatment, and the low temperature tempering heat treatment prevents cracking of the coating or components of the high alloy material. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is a flow chart of the method and application of the present invention;

[0033] Figure 2 The X-ray diffraction pattern of the high alloy high speed steel metal powder of the present invention;

[0034] Figure 3 The backscattered scanning electron microscope images of the cross section of the high-speed steel powder of the present invention, (a) untreated powder; (b) treated powder;

[0035] Figure 4 This is a macroscopic physical picture of the test of the effect of heat treatment temperature on the sintering characteristics of powders in the present invention;

[0036] Figure 5 This is a backscattered scanning electron image of the untreated metal powder laser cladding coating of the present invention;

[0037] Figure 6 The backscattered scanning electron image and element energy spectrum of the phase change powder laser cladding coating of the present invention, (a) the junction between the cladding layer and the substrate; (b) the microstructure of the cladding layer. DETAILED DESCRIPTION

[0038] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the following will be combined with the appended drawings of the embodiments of the present invention. Figure 1-6 , the technical scheme of the embodiment of the present invention is clearly and completely described. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.

[0039] Embodiment 1

[0040] Phase transformation heat treatment of metal powders containing carbide-forming elements;

[0041] (1) High alloy high speed steel powder is selected as the metal powder. The metal powder contains relatively high carbide synthesis elements C, V, W, Mo and Cr. The chemical composition and mass percentage are as follows:

[0042] C: 1.5~1.8, W: 9.0~11.0, Mo: 2.0~4.0, Cr: 4.0~6.0, V: 4.0~6.0, Si: 0.2~0.5, S: ≤0.02, P: ≤0.02.

[0043] The metal powder has a sieved average particle size D50 of 45-65μm and a fluidity of 20s / 50g.

[0044] The metal powder is contained in a 316L stainless steel tank filled with argon gas, and then the tank is sealed.

[0045] (2) Place the sealed can body in a heat treatment furnace filled with argon atmosphere, with argon atmosphere protection throughout the process, the heating rate is 10℃ / min, the insulation temperature is 890~910℃, the insulation time is 64~72 hours, and then cool to room temperature after taking out.

[0046] Metal powders that have undergone phase change heat treatment can be applied to the field of additive manufacturing, including but not limited to layer-by-layer accumulation through extrusion, sintering, melting, photocuring, spraying, etc., to produce physical objects. The following is a detailed implementation of the laser cladding method to coat the workpiece with a hard and wear-resistant coating;

[0047] (3) Use a 9Cr2Mo metal round bar workpiece with a diameter of 40 mm, grind and polish the surface of the workpiece, wipe it with ethanol to remove surface grease and metal residue, and preheat the cleaned workpiece to 300°C.

[0048] (4) The phase change metal powder is clad on the surface treated part to be clad by laser cladding. The process parameters of laser cladding are: 2100W, laser radius of 1.2mm, scanning speed of 3mm / s, overlap rate of 40%, powder feeding rate of 4r / min, and argon flow rate of 5L / min. After cladding, the clad part is immediately placed in a heat treatment furnace, the heating step rate is 10℃ / min, the insulation temperature is 550-560℃, and the insulation time is 1 hour each time. It is tempered 3 times in the temperature range of 550-560℃, and the furnace is cooled to room temperature to obtain an additively manufactured object coated with a cladding layer.

[0049] Embodiment 2

[0050] The difference between this embodiment and the first embodiment lies in step (2), placing the sealed can body into a heat treatment furnace filled with argon atmosphere, with argon atmosphere protection throughout the whole process, the heating step rate is 10°C / min, the insulation temperature is 530-560°C, the insulation time is 32 hours, and then cooling to room temperature after taking out.

[0051] Embodiment 3

[0052] The difference between this embodiment and the first embodiment is that (2) the sealed can body is placed in a heat treatment furnace filled with argon atmosphere, and the argon atmosphere is protected throughout the process. The heating rate is 10°C / min, the insulation temperature is 820-840°C, the insulation time is 32 hours, and it is taken out and cooled to room temperature.

[0053] Comparative Example 1

[0054] Phase transformation heat treatment of metal powders containing carbide-forming elements;

[0055] (1) The metal powder is selected from high-alloy high-speed steel powder, which contains high carbide synthesis elements (C, V, W, Mo and Cr). The chemical composition and mass percentage of the powder high-speed steel powder are: C: 1.5-1.8, W: 9.0-11.0, Mo: 2.0-4.0, Cr: 4.0-6.0, V: 4.0-6.0, Si: 0.2-0.5, S: ≤0.02, P: ≤0.02. The average particle size D50 of the metal powder after screening is 45-65μm, and the fluidity is 21s / 50g. The metal powder is contained in a 316L stainless steel tank filled with argon gas, and then the tank is sealed.

[0056] (2) Place the sealed tank into a heat treatment furnace filled with argon atmosphere, and protect it with argon atmosphere throughout the process without heating or cooling operations. The duration is 64 to 72 hours.

[0057] Metal powders that have undergone phase change heat treatment can be applied to the field of additive manufacturing, including but not limited to layer-by-layer accumulation through extrusion, sintering, melting, photocuring, spraying, etc., to produce physical objects. The following is a detailed implementation of the laser cladding method to coat the workpiece with a hard and wear-resistant coating;

[0058] (3) In this example, a 9Cr2Mo metal round bar with a diameter of 40 mm is used. 9Cr2Mo material is mainly used for wear-resistant rollers, rolling rollers, cold stamping dies and punches. The surface of the workpiece or substrate is ground and polished, and ethanol is used to wipe off the surface grease and metal residues. The cleaned workpiece or substrate to be clad is preheated to 300°C.

[0059] (4) The phase change metal powder is clad on the surface treated part to be clad by laser cladding. The process parameters of laser cladding are: 2100W, laser radius of 1.2mm, scanning speed of 3mm / s, overlap rate of 40%, powder feeding rate of 4r / min, and argon flow rate of 5L / min. After cladding, the clad part is immediately placed in a heat treatment furnace, the heating step rate is 10℃ / min, the insulation temperature is 550-560℃, and the insulation time is 1 hour each time. It is tempered 3 times in the temperature range of 550-560℃, and the furnace is cooled to room temperature to obtain an additively manufactured object coated with a cladding layer.

[0060] Comparative Example 2

[0061] (1) The metal powder is selected from high alloy high speed steel powder, which contains high carbide synthesis elements (C, V, W, Mo and Cr). The chemical composition and mass percentage of the powder high speed steel powder are: C: 1.5-1.8, W: 9.0-11.0, Mo: 2.0-4.0, Cr: 4.0-6.0, V: 4.0-6.0, Si: 0.2-0.5, S: ≤0.02, P: ≤0.02. The average particle size of the metal powder after screening is D 50 The particle size is 45-65 μm, the fluidity is 21 s / 50 g, and the metal powder is directly loaded into an alumina crucible, with a small amount of argon gas for protection and some residual air.

[0062] (2) Place 8 alumina crucibles containing the same powder in a heat treatment furnace at a heating rate of 10°C / min and take them out when they reach the desired temperature or reach the desired time at 200°C, 400°C, 600°C, 800°C, 1000°C, 1200°C, 1200°C (1 hour) and 1200°C (2 hours).

[0063] (3) By sampling and analyzing the fluidity state of the powder at different heat treatment temperatures, Figure 4The figure shows the macroscopic physical picture of the test of the effect of heat treatment temperature on the sintering characteristics of powder. The powder samples heat treated below 1000°C are in powder form and are obtained by pouring out by tilting the crucible. The powder samples heat treated above 1000°C are in round cake-shaped blocks and are obtained by smashing the alumina crucible, that is, sintering occurs. Based on the requirements of powder raw materials for additive manufacturing processes, powder fluidity and powder particle size distribution, powder sintered into blocks cannot be used for additive manufacturing. In addition, the alloy powder surface appears reddish-brown when the powder is heat treated at 600°C without atmosphere protection. General scientific knowledge shows that ferric oxide (rust) is generated. Oxidized metal powders also do not meet the requirements of powder raw materials for additive manufacturing processes (low oxygen content).

[0064] analyze:

[0065] The metal powder sampling and analysis during the heat treatment in step (2) of Example 1 showed that the fluidity of the metal powder sampled after 4 hours was 20 s / 50 g, the fluidity of the metal powder sampled after 8 hours was 21 s / 50 g, the fluidity of the metal powder sampled after 16 hours was 20 s / 50 g, the fluidity of the metal powder sampled after 64 hours was 23 s / 50 g, and the fluidity of the metal powder sampled after 72 hours was 22 s / 50 g. The fluidity of the metal powder did not change significantly during the heat treatment time.

[0066] like Figure 2 As shown, the metal powder in Example 1 exhibits obvious precipitation of M6C type carbide phase after heat treatment.

[0067] like Figure 3 As shown, Figure 3 -a is the original alloy powder characterized by MC-type dendrite carbides, Figure 3 -b shows that there are more granular phases with a diameter of 0.5 to 2 μm precipitated. Combined with the X-ray diffraction results, it shows that granular MC and M6C carbides precipitate in large quantities during the heat treatment process.

[0068] After microhardness testing, the hardness of the metal powder after heat treatment in Example 1 was increased to 817.8 HV 0.3 (64.6HRC).

[0069] The cross section of the cladding part of Example 1 was sampled, and after metallographic sample preparation, optical microscope and scanning electron microscope structure analysis were performed, and it was found that granular carbides still existed in the coating.

[0070] The Vickers microhardness test of Example 1 shows that the hardness of the powder cladding layer after heat treatment is 811.3 HV 0.3 (64.4HRC), the present invention can significantly improve the hardness of the cladding coating.

[0071] The difference between Example 2 and Example 1 is that a temperature close to the lowest heat treatment temperature (500°C) is used to illustrate that heat treatment in this temperature range has a certain effect. Vickers microhardness test is performed, and the hardness of the powder cladding layer after heat treatment is 709.0 HV 0.3 (61.3HRC), the second embodiment can improve the hardness of the cladding coating to a certain extent.

[0072] The difference between Example 3 and Example 1 is that a heat treatment temperature close to the middle of the temperature range (725°C) is used. The purpose is also to show that the heat treatment in this temperature range is effective. The Vickers microhardness test shows that the hardness of the powder cladding layer after heat treatment is 758.5HV. 0.3 (62.8HRC), this embodiment can improve the hardness of the cladding coating to a certain extent.

[0073] By sampling and analyzing the heat-treated metal powder in Comparative Example 1, the fluidity of the metal powder is 21s / 50g, and the hardness of the original metal powder is 564.9HV after microhardness test. 0.3 (53.3HRC).

[0074] like Figure 2 As shown, the original powder only contains MC type carbides.

[0075] like Figure 3 As shown, Figure 3 The original powder has only dendrite carbides of about 200 nm in size, and the alloy elements in the original powder cannot form more M6C carbides due to rapid cooling.

[0076] The cross section of the cladding part of comparative example 1 was sampled and subjected to optical microscope and scanning electron microscope structure analysis after metallographic sample preparation. Figure 5 As shown, there are more dendrite carbides in the coating. According to the Vickers microhardness test, the hardness of the untreated powder cladding layer is 638.8HV 0.3 (57.3HRC).

[0077] Through the analysis of Example 2, Figure 4 As shown, Figure 4 a~d in the figure are still powdery after heat treatment. Figure 4 In the figure, e~h, the powders after heat treatment appear as sintered blocks, that is, there is a reasonable temperature range below 1000°C where the heat-treated powders will not sinter to form blocks, which serves as additional evidence for the rationality of the selection of the upper limit range of the heat treatment temperature.

[0078] Heat treatment below 500°C has no significant effect on the microstructure of the alloy powder, and the slow phase transformation has no practical significance and is not conducive to energy conservation and environmental protection.

[0079] Table 1 shows the differences in organization and performance between the examples and the comparative examples. After the metal powder is heat treated, combined with XRD and microstructure analysis, the carbide phase shows obvious precipitation behavior, especially the M6C type carbide in the form of granules. Through the metal powder hardness test, the increase in the hardness of the metal powder after heat treatment is related to the precipitation of the carbide phase.

[0080] Through microstructural observation, as shown in the figure, the cladding layer of comparative example 1 still presents a network of carbides, and the cladding layer of embodiment 1 presents granular carbides. The hardness of the metal powder cladding layer after heat treatment (811.3 HV 0.3 ) is much higher than the hardness of the untreated metal powder cladding layer (638.8HV 0.3 ), which is mainly related to the large amount of carbides precipitated in the metal powder after heat treatment, and the microstructure type of some metal powders is inherited during laser cladding.

[0081] In comparative example 1, the hardness of the cladding layer is significantly higher than that of the powder, which may be related to the three tempering processes. It has been reported in the literature that the tempering process will promote the precipitation of nano-scale carbide phases and thus increase the hardness. Figure 3 b and Figure 5 b. The bright white granular W-rich carbides precipitated in the powder are transformed into rod-shaped carbides after laser cladding, while the gray granular carbides precipitated in the powder do not change significantly. The main reason is related to the high temperature generated during laser cladding. When the metal powder is melted quickly, the bright white W-rich carbides will decompose and dissolve back. When the metal cladding layer is cooled quickly, the white W-rich carbides cannot be completely precipitated again. Therefore, the hardness of the cladding layer is slightly lower than that of the metal powder after heat treatment.

[0082] In summary, the present invention can be applied in the field of additive manufacturing through metal powder phase change technology, and can significantly improve the hardness of additively manufactured workpieces or coatings.

[0083] Table 1 Differences in organization and performance between the examples and the comparative examples

[0084]

[0085] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing phase change metal powder for workpiece coating, characterized in that: The following steps are involved: The high-alloy high-speed steel powder is placed in a high-temperature resistant tank in an isolated environment, wherein the chemical composition and mass percentage of the high-alloy high-speed steel powder are as follows: C: 1.5-1.8%, W: 9.0-11.0%, Mo: 2.0-4.0%, Cr: 4.0-6.0%, V: 4.0-6.0%, Si: 0.2-0.5%, S: ≤0.02%, P: ≤0.02%; the high-alloy high-speed steel powder is heat-treated at 820-910° C. for 32-72 hours; and the powder is taken out and cooled to room temperature to obtain a phase change metal powder; The method for using the phase change metal powder for workpiece coating comprises the following steps: S1. Surface treatment is performed on the parts to be clad, and preheating is performed in the temperature range of 250-350℃; S2. The phase change metal powder is clad on the surface treated workpiece to be clad by laser cladding, wherein the process parameters of the laser cladding are: 1500-3000W, laser radius of 0.5-1.5mm, scanning speed of 5-50mm / s, overlap rate of 20-80%, powder feeding rate of 2-50r / min, and argon flow rate of 3-15L / min; S3, tempering the cladding part at a temperature range of 520-560° C. for 1-3 times to obtain an additively manufactured workpiece.

2. The method for preparing phase change metal powder for workpiece coating according to claim 1, characterized in that: The heating rate of the high alloy high speed steel powder during heat treatment is not higher than 10° C. / min.

3. The method for preparing phase change metal powder for workpiece coating according to claim 1, characterized in that: The isolated environment is a protective atmosphere or a vacuum environment.

4. The method for preparing phase change metal powder for workpiece coating according to claim 1, characterized in that: The phase content of the cladding layer changes, and the change in phase content is manifested in an increase in carbide precipitation.

5. The method for preparing phase change metal powder for workpiece coating according to claim 1, characterized in that: The hardness of the cladding layer is 55-65hrc.

6. The method for preparing phase change metal powder for workpiece coating according to claim 1, characterized in that: The fluidity of the phase change metal powder subjected to laser cladding is 20 to 45 s / 50 g.

7. The phase change metal powder prepared by the preparation method according to any one of claims 1 to 6 is used in additive manufacturing.

Citation Information

Patent Citations

  • Laser cladding material of 42CrMo gear ring as well as laser cladding method and application

    CN113265656A

  • Iron-based laser cladding material and wear-resistant iron-based laser cladding layer

    CN115673314A

  • Precursor carbonization plasma cladding reaction synthesized WC reinforced metal based alloy coating and preparation

    CN103382555A

  • Powder for laser cladding in-situ self-generated vanadium carbide reinforced iron-based alloy and preparation method

    CN108339976A

  • Laser-cladding in-situ synthesized carbide-particle-reinforced iron-based cladding layer and preparing method thereof

    CN111607789A