Aluminum-carbon composite material based on stir friction deposition additive and preparation method thereof

Through friction stir deposition additive technology and post-treatment technology, the problems of low density and serious interface reaction in the preparation of traditional aluminum-carbon composite materials were solved, and high-performance aluminum-carbon composite materials were obtained, which were suitable for aerospace structural parts.

CN116213749BActive Publication Date: 2024-11-08BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310023754.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-09
Publication Date
2024-11-08
Estimated Expiration
2043-01-09

AI Technical Summary

Technical Problem

The traditional aluminum-carbon composite preparation process has problems such as low density, long preparation time, serious high-temperature interface reactions and poor enhanced phase dispersion, which is difficult to meet the high strength and high thermal conductivity requirements of aerospace materials.

Method used

Using friction stir deposition additive technology, the composite powder of aluminum powder/carbon powder is obtained by mixing powder, and the forming materials are prepared through friction stir deposition additive process, combining turning processing and post-heat treatment to optimize the thickness and process of friction stir additive layer Parameters, satisfy specific formula conditions to improve material performance.

Benefits of technology

The obtained aluminum-carbon composite material has low residual stress, small grains, few interfacial reactions, good enhanced phase dispersion, good matching of elastic modulus and strong plasticity. It is suitable for aerospace structural parts, and its performance exceeds traditional processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116213749B_ABST
    Figure CN116213749B_ABST
Patent Text Reader

Abstract

The present invention relates to a preparation process of aluminum-carbon composite materials based on stir friction deposition additive, comprising the following steps: (1) obtaining aluminum powder / carbon powder composite powder by mixing powder; (2) obtaining block material by stir friction deposition additive deposition of the composite powder; (3) turning and post-heat treatment of the block material. Compared with the prior art, the present invention can directly obtain aluminum-carbon composite parts and block materials with good dispersion of reinforcement phase, less generation of interface brittle products and low residual stress, thereby giving full play to the reinforcement effect of carbon phase.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of friction stir additives and relates to an aluminum-carbon composite material based on friction stir deposition additives and a preparation method thereof. Background Art

[0002] For aluminum-carbon composite materials, the traditional preparation process is hot pressing sintering-extrusion deformation, but this process has problems such as low density, long preparation time, severe high-temperature interface reaction and poor dispersion of the reinforcing phase, which leads to the mechanical properties of the material failing to meet expectations.

[0003] Friction stir deposition additive technology was first reported by MELD in the United States. It uses rods or powders as raw materials. Under the action of extrusion force, the material is squeezed into the friction stir head, and the solid phase additive manufacturing of the block is realized under the conditions of friction heat and plastic deformation. The parts obtained by this method have the advantages of low residual stress and fine grains.

[0004] At present, the stir friction deposition additive technology with powder as feed is limited to aluminum alloy powder, and its powder is directly atomized powder. However, the use of traditional atomized alloy powder is difficult to meet the high strength, high modulus or high thermal conductivity requirements of aerospace materials. Summary of the invention

[0005] In view of the above problems existing in the prior art, the present invention provides an aluminum-carbon composite material based on stir friction deposition additive and a preparation method thereof.

[0006] The complete technical solution of the present invention is:

[0007] A method for preparing an aluminum-carbon composite material based on stir friction deposition additive, comprising the following steps:

[0008] (1) obtaining a composite powder of aluminum powder / carbon powder by mixing powder;

[0009] (2) for the composite powder obtained in step (1), adding material by friction stir deposition to obtain a molding material;

[0010] (3) Subsequent processing of the molding material obtained in step (2)

[0011] Furthermore, the powder mixing in step (1) is a powder mixing process using mechanical ball milling, a mixer, liquid phase stirring, or a combination of the above processes.

[0012] Furthermore, the mass percentage of carbon powder in the composite powder of step (1) is greater than 0 and not higher than 15%.

[0013] Furthermore, the carbon powder in step (1) is carbon nanotube powder, graphene powder, graphite powder, or a combination of the above powders.

[0014] Furthermore, the carbon nanotubes are single-walled carbon nanotubes, multi-walled carbon nanotubes, or a combination of the above materials; the graphene is single-layer graphene, multi-layer graphene, oxidized graphene, modified graphene, or a combination of the above materials.

[0015] Furthermore, the powder feeding method of the stir friction deposition additive in step (2) includes but is not limited to screw powder feeding and extrusion rod powder feeding.

[0016] Furthermore, the thickness of the friction stir additive layer is 0.1 to 2 mm, and the preferred thickness of the friction stir additive layer is d 碳素 The friction stir deposition additive process parameters and the carbon content x (wt.%) satisfy the formula (1):

[0017]

[0018] Where P is the shoulder compressive stress in MPa, ω is the stirring head speed in RPM, v is the stirring head moving speed in mm / min, d1 is the average particle size of aluminum powder after ball milling in mm, SA is the carbon relative surface area in m 2 / g, A1 is the correction factor related to heat generation and stirring head morphology, and its value range is 0.001~1mm 2 , A2 is the correction factor related to interface energy, and its value range is 1~2000mJ / m 2 , ρ is the density of aluminum powder, unit is g / m 3 , ρ1 is the density of the composite material, in g / m 3 , x is the mass percentage of carbon powder in the composite powder, in wt.%.

[0019] Furthermore, when the mechanical parameters of friction stir additive, such as the shoulder pressure, the stirring head speed, the stirring head moving speed and the average particle size of the aluminum powder after ball milling are fixed, the preferred additive layer thickness d of the aluminum-carbon composite material with a carbon content of x is ′ 碳素 Thickness of pure aluminum friction stir additive layer d 纯铝 Satisfies formula (2):

[0020]

[0021] Furthermore, the post-processing includes turning and post-heat treatment, and the heat treatment temperature does not exceed 450°C.

[0022] Furthermore, the aluminum-carbon composite material has a tensile strength of not less than 280.5 MPa, an elongation of not less than 16.0%, and an elastic modulus of not less than 78 GPa.

[0023] The advantages of the present invention over the prior art are:

[0024] The preparation method is suitable for preparing aluminum-carbon composite parts. The obtained aluminum-carbon composite material has less interface reaction, good dispersion of reinforcing phase, designable elastic modulus and good matching of strength and plasticity. It has important potential application value in important structural parts such as aviation and aerospace. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the basic process flow of the present invention.

[0026] Figure 2 This is a picture of the composite powder microstructure. DETAILED DESCRIPTION

[0027] The present invention is described in detail below in conjunction with the embodiments and drawings, but it should be understood that the embodiments and drawings are only used to exemplify the present invention and do not constitute any limitation on the protection scope of the present invention. All reasonable changes and combinations within the scope of the inventive concept of the present invention fall within the protection scope of the present invention.

[0028] like Figure 1 As shown, the present invention discloses a method for preparing an aluminum-carbon composite material based on stir friction deposition additive. It includes:

[0029] (1) A composite powder of aluminum powder / carbon powder is obtained by mixing powders in a mechanical ball mill, a mixer, a liquid phase stirring powder, or the like; the carbon powder can be single-walled carbon nanotubes, multi-walled carbon nanotubes, or a combination of the above materials; the graphene can be single-layer graphene, multi-layer graphene, oxidized graphene, modified graphene, or the like, or a combination of the above materials;

[0030] (2) for the composite powder obtained in step (1), adding material by friction stir deposition to obtain a bulk material;

[0031] During the experiment, it was found that as the carbon phase content increases, the processing can only be carried out smoothly by increasing the rotation speed of the stirring head, or reducing the moving speed of the stirring head, or reducing the thickness of the single-layer additive layer. This is because the carbon phase itself has a large specific surface area and its wettability with the aluminum matrix is ​​poor, so it is necessary to provide a higher energy input per unit time, otherwise it will cause the additive block to crack and the powder to not be welded. At the same time, due to the large differences in the specific surface properties and interface properties of different types of carbon phases, it is difficult to coordinate the processing parameters. Based on the above problems, the use of formulas (1) and (2) can more intuitively guide the processing parameters of composite powders with different contents and types of carbon phases.

[0032] The thickness of the friction stir additive layer is 0.1 to 2 mm. The preferred thickness of the friction stir additive layer is d 碳素The friction stir deposition additive process parameters and the carbon content x (wt.%) satisfy the formula (1):

[0033]

[0034] Where P is the shoulder pressure stress, unit is MPa, ω is the stirring head speed, unit is RPM, v is the stirring movement speed, unit is mm / min, d1 is the average particle size of aluminum powder after ball milling, unit is mm, SA is the carbon relative surface area, unit is m 2 / g, A1 is the correction factor related to heat generation and stirring head morphology, and its value range is 0.001~1mm 2 , A2 is the correction factor related to interface energy, and its value range is 1~2000mJ / m 2 , ρ is the density of aluminum powder, unit is g / m 3 , ρ1 is the density of the composite material, in g / m 3 , x is the mass percentage of carbon powder in the composite powder, in wt.%.

[0035] Among them, when the mechanical parameters of stir friction additive are fixed, such as the shoulder pressure, the stirring head speed, the stirring head moving speed and the average particle size of the aluminum powder after ball milling, the preferred additive layer thickness d of the aluminum-carbon composite material with a carbon content of x is ′ 碳素 Thickness of pure aluminum friction stir additive layer d 纯铝 Satisfies formula (2):

[0036]

[0037] (3) The block material obtained in step (2) is subjected to turning and post-heat treatment, wherein the heat treatment temperature does not exceed 450°C.

[0038] Example 1

[0039] (1) obtaining a composite powder of graphene nanosheets with a carbon content of 0.3 wt.% and aluminum powder; wherein the aluminum powder has a particle size of 460 mesh, and the graphene nanosheets have a sheet diameter of 1 to 3 microns and a thickness of 3 to 10 nm;

[0040] 99.7 g aluminum powder and 0.3 g graphene nanosheets were ball-milled at a speed of 250 rpm for 8 h and a ball-to-material ratio of 5:1 to obtain a composite powder. The composite powder was placed in an argon environment for 2 days. The powder morphology is as follows: Figure 2 shown.

[0041] (2) Friction stir deposition is carried out according to the designed process, and the composite powder is passed through the friction stir deposition equipment to obtain an additive block, and the additive layer thickness is 0.5 mm.

[0042] (3) Heat treatment of the additive block at 300 °C for 2 h.

[0043] Example 2

[0044] (1) obtaining a composite powder of graphene nanosheets with a carbon content of 0.5 wt.% and aluminum powder, wherein the aluminum powder has a particle size of 460 mesh, the graphene nanosheets have a sheet diameter of 1 to 3 microns, and a thickness of 3 to 10 nm;

[0045] Take 99.5g aluminum powder for preliminary ball milling, the ball milling speed is 350rpm, the ball milling time is 8h, and the ball-to-material ratio is 10:1.

[0046] Take 0.5 g of graphene nanosheets and add them to the previously ball-milled aluminum powder. The ball milling speed is 250 rpm, the ball milling time is 10 h, and the ball-to-material ratio is 5:1 to obtain a composite powder. The composite powder is placed in an argon environment for 2 days.

[0047] (2) The composite powder is subjected to friction stir deposition to obtain an additive block, and the additive layer thickness is 0.35 mm.

[0048] (3) Heat treatment of the additive block at 300 °C for 2 h.

[0049] Example 3

[0050] (1) obtaining a composite powder of carbon nanotubes with a carbon content of 0.5 wt.% and aluminum powder, wherein the aluminum powder has a particle size of 460 mesh, and the carbon nanotubes are multi-walled carbon nanotubes with a diameter of 5 to 15 nm and a length of 0.5 to 2 microns;

[0051] First, take 200g of aluminum powder for preliminary ball milling, the ball milling speed is 350rpm, the ball milling time is 8h, and the ball-to-material ratio is 10:1; then take 0.5g of carbon nanotubes and add them to 200ml of anhydrous ethanol solution for ultrasonic dispersion for 1h; take 99.5g of the ball-milled aluminum powder and add it to 200ml of anhydrous ethanol solution and stir it magnetically, add the carbon nanotube dispersion to the aluminum powder solution, continue magnetic stirring, and the stirring temperature is 50℃. After all the anhydrous ethanol is evaporated, put the composite powder into a vacuum drying oven for drying.

[0052] (2) The composite powder is subjected to a friction stir deposition device to obtain an additive block, and the additive layer thickness is 0.35 mm.

[0053] (3) Heat treatment of the additive block at 250 °C for 2 h.

[0054] Example 4

[0055] (1) A composite powder of graphite powder and aluminum powder with a carbon content of 5 wt.% was obtained, wherein the average particle size of the aluminum powder was 10 μm, the average particle size of the graphite powder was 1 μm, and the specific surface area was 18 m 2 / g;

[0056] Take 95g aluminum powder and 5g graphite powder and add them into a Y-type mixer for 12h;

[0057] (2) The composite powder is subjected to friction stir deposition to obtain an additive block, and the additive layer thickness is 0.5 mm.

[0058] (3) Heat treatment of the additive block at 250 °C for 2 h.

[0059] Example 5

[0060] (1) A composite powder of graphite powder and aluminum powder with a carbon content of 10 wt.% was obtained, wherein the average particle size of the aluminum powder was 10 μm, the average particle size of the graphite powder was 1 μm, and the specific surface area was 18 m 2 / g;

[0061] Take 90g aluminum powder and 10g graphite powder and add them into a Y-type mixer. Mix for 12h.

[0062] (2) The composite powder is subjected to friction stir deposition to obtain an additive block, and the additive layer thickness is 0.3 mm.

[0063] (3) Heat treatment of the additive block at 250 °C for 2 h.

[0064] Comparative Example

[0065] (1) Take 100 g of pure aluminum powder, wherein the particle size of the aluminum powder is 460 mesh;

[0066] (2) Pure aluminum powder is deposited by friction stir deposition equipment with a thickness of 1.2 mm.

[0067] (3) Heat treatment of the additive block at 300 °C for 2 h.

[0068] Table 1 Performance index comparison

[0069] Serial number Element Strength / MPa Elongation / % Elastic modulus / GPa Example 1 0.3wt.%GNPS / Al 230.6 16.0 75 Example 2 0.5wt.%GNPS / Al 280.5 12.6 78 Example 3 0.5wt.%CNTS / Al 255.6 13.5 77 Example 4 5wt.%Graphite / Al 160.4 8.5 67 Example 5 10wt.%Graphite / Al 175.5 5.2 64 Comparative Example Pure Al 120 12 71

[0070] Table 1 is a performance comparison between aluminum-carbon composite materials and pure aluminum obtained by selecting different components, according to different carbon contents, stir friction deposition additive mechanical parameters and layer thicknesses in a specific implementation manner. It can be seen that, compared with pure aluminum materials, the aluminum-carbon composite materials obtained in the present invention have obvious improvements in strength, elongation and elastic modulus, and the preparation method disclosed in the present invention is very suitable for preparing aluminum-carbon composite parts. The obtained aluminum-carbon composite materials have less interface reaction, good dispersion of reinforcing phase, designable elastic modulus and good matching of strength and plasticity, and have important potential application value in important structural parts such as aviation and aerospace.

[0071] The above applications are only some implementation methods of the present application. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present application, and these all belong to the protection scope of the present application.

Claims

1. A method for preparing aluminum-carbon composite materials based on stir friction deposition additive, It is characterized in that The following steps are involved: (1) Obtaining aluminum powder / carbon powder composite powder by mixing powder; (2) for the composite powder obtained in step (1), adding material by stir friction deposition to obtain a molding material; The thickness of the friction stir additive layer is 0.1~2mm. The friction stir deposition additive process parameters and the carbon content x satisfy the formula (1): (1) In the formula, is the shoulder compressive stress, in MPa, is the stirring head speed, in RPM, v is the stirring head moving speed, in mm / min, d 1 is the average particle size of aluminum powder after ball milling, in mm, SA is the relative surface area of ​​carbon, in m 2 / g,A 1 is the correction factor related to heat generation and stirring head morphology, with a value range of 0.001~1 mm 2 , A 2 is the correction factor related to the interface energy, ranging from 1 to 2000 mJ / m 2 , is the density of aluminum powder, in g / m 3 , 1 is the density of the composite material, in g / m 3 , x is the mass percentage of carbon powder in the composite powder, unit is wt.%; (3) Performing subsequent processing on the molding material obtained in step (2).

2. A method for preparing an aluminum-carbon composite material based on stir friction deposition additive according to claim 1, It is characterized in that The powder mixing in step (1) is a powder mixing process using mechanical ball milling, a mixer, liquid phase stirring, or a combination of the above processes.

3. The method for preparing an aluminum-carbon composite material based on stir friction deposition additive according to claim 1, It is characterized in that The mass percentage of carbon powder in the composite powder of step (1) is greater than 0 and not higher than 15%.

4. The method for preparing an aluminum-carbon composite material based on stir friction deposition additive according to claim 1, It is characterized in that The carbon powder in step (1) is carbon nanotube powder, graphene powder, graphite powder, or a combination of the above powders.

5. A method for preparing an aluminum-carbon composite material based on stir friction deposition additive according to claim 4, It is characterized in that The carbon nanotubes are single-walled carbon nanotubes, multi-walled carbon nanotubes, or a combination of the above materials; the graphene is single-layer graphene, multi-layer graphene, oxidized graphene, modified graphene, or a combination of the above materials.

6. The method for preparing an aluminum-carbon composite material based on stir friction deposition additive according to claim 1, It is characterized in that The powder feeding method of the stir friction deposition additive in step (2) includes but is not limited to screw powder feeding and extrusion rod powder feeding.

7. The method for preparing an aluminum-carbon composite material based on stir friction deposition additive according to claim 1, It is characterized in that When the mechanical parameters of friction stir additive are fixed, such as the shoulder pressure, the speed of the stirring head, the moving speed of the stirring head and the average particle size of the aluminum powder after ball milling, the thickness of the friction stir additive layer of the aluminum-carbon composite material with a carbon content of x is Thickness of pure aluminum friction stir additive layer Satisfies formula (2): (2)。 8. The method for preparing an aluminum-carbon composite material based on stir friction deposition additive according to claim 1, It is characterized in that The subsequent processing in step (3) is turning and post-heat treatment, and the heat treatment temperature does not exceed 450°C.

9. The aluminum-carbon composite material obtained according to the method according to any one of claims 1 to 8.