Ultralow-yield-ratio high-phosphorus atmospheric corrosion-resistant steel and preparation method thereof
By using low-carbon and low-cost phosphorus and chromium alloy elements in weathering steel, combined with two-stage rolling and microalloyization processes, the problem of high consumption of valuable elements in weathering steel is solved, and high toughness, high corrosion resistance and low cost are achieved. Ultra-low yield strength ratio high phosphorus resistant atmospheric corrosion steel, suitable for bridges and building structures.
Patent Information
- Application Number
- CN202411000141.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The existing weathering steel has a large amount of precious elements, high production costs, and a high yield ratio affects the safety and seismic resistance of bridges.
Low-carbon components are used to add low-cost phosphorus and chromium alloy elements, and the corrosion resistance of materials is improved through small, uniform structure and phosphorus and chromium compounds. Two-stage rolling and microalloying processes are adopted to control chemical compositions at C 0.05%~0.07% , Si 0.10%~0.20%, Mn 1.20%~1.35%, P 0.060%~0.080%, Cr ≤0.80%, Cu ≤0.50%, Ni ≤0.50%, Ti ≤0.020%, to meet high toughness and high corrosion resistance , easy welding requirements.
Reduces the amount of precious elements, improves the weather resistance and comprehensive mechanical properties of the material, and reduces production costs. The steel plate has excellent strong plastic matching, welding performance and low yield and strength ratio, and has an increase of more than 1.5 times weather resistance, suitable for coating-free Buildings and bridge structures.
Smart Images

Figure CN119040738A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to an ultra-low yield ratio high-phosphorus atmospheric corrosion resistant steel and a preparation method thereof. Background Art
[0002] Steel plates exposed to air for a long time will be damaged by corrosion. The cost of anti-corrosion accounts for a large proportion of the later maintenance costs of buildings and steel bridges. Steel plates with excellent corrosion resistance do not need to be painted under certain conditions, which can greatly reduce the operation and maintenance costs of steel structures and have significant economic and environmental effects. Therefore, corrosion-resistant steel has significant advantages over ordinary steel in the application of large-scale steel structure projects such as bridges and building structures.
[0003] Chinese patent application CN 109161793 A discloses a low yield ratio high strength weathering steel. The finished product obtained by this method has a thickness of 6 to 12 mm, a relatively thin thickness specification, and a narrow application range. Precious elements such as Cu, Ni, Cr, Nb and Ti must be used simultaneously, and the alloy cost is high.
[0004] Chinese patent application CN 113201687 A discloses a 420MPa weather-resistant bridge steel, whose chemical composition and mass percentage are: C 0.05%~0.07%, Si 0.25%~0.50%, Mn 1.10%~1.70%, P≤0.020%, S≤0.010%, Cu 0.28%~0.35%, Ni 0.20%~0.30%, Cr 0.45%~0.55%, Mo≤0.10%, Nb 0.008%~0.030%, Ti 0.010%~0.030%, V 0.005%~0.015%, Als 0.020%~0.035%, Ca 0.0020%~0.0050%, O≤0.0040%, N 0.0025%~0.0080%, the balance is Fe and unavoidable impurities. The alloy composition of this weather-resistant bridge steel is complex and the production cost is high. In addition, the yield strength of this weather-resistant bridge steel is relatively high, between 0.78~0.82, which has a great impact on the safety and earthquake resistance of the bridge. Summary of the invention
[0005] In view of the technical problems that weathering steel uses a large amount of precious elements, has a high production cost, and has a high yield ratio of the finished steel, the present invention provides an ultra-low yield ratio high-phosphorus atmospheric corrosion resistant steel and a preparation method thereof, which adopts a lower carbon component, adds cheap phosphorus and chromium alloy elements, and utilizes fine and uniform structure and phosphorus and chromium compounds to improve the corrosion resistance of the material, so that the material has high toughness, high corrosion resistance, and easy welding capabilities, thereby meeting the corrosion resistance and high toughness requirements of steel for building structures and engineering structures in coastal atmospheric environments.
[0006] In a first aspect, the present invention provides a method for preparing an ultra-low yield ratio high-phosphorus atmospheric corrosion resistant steel, wherein the chemical composition and weight percentage of the ultra-low yield ratio high-phosphorus atmospheric corrosion resistant steel are C: 0.05% to 0.07%, Si: 0.10% to 0.20%, Mn: 1.20% to 1.35%, 0.060%≤P≤0.080%, S≤0.003%, Als: 0.010% to 0.040%, Cr≤0.80%, Cu≤0.50%, Ni≤0.50%, Ti≤0.020%, and the balance is Fe and unavoidable impurities; The preparation method comprises at least the following steps: Put the cut ingot into the slow cooling pit, the starting slow cooling temperature of the ingot is ≥500℃, and the ending slow cooling temperature is not less than 300℃; Heat the slowly cooled ingot, control the ingot out-of-furnace temperature to be 1140~1170℃, and the furnace time coefficient to be 10~11min / cm; Two-stage rolling is adopted. The first stage rolling is carried out after the billet is descaled. When the second stage rolling starts, the surface temperature of the rolled piece is T2=(T+1600 / H-1.8H)℃, where T=870+11.2[%C]-1.8[%Si]+18[%Mn]+1.6[%Al]-1.2[%Cr], H is the thickness of the steel plate in mm, and the steel plate is not water-cooled after rolling; After rolling, the steel plate is placed in a pile cooling room at 500~600℃ for no less than 48 hours.
[0007] Furthermore, the chemical composition of the ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel satisfies the marine atmospheric corrosion resistance index of 1.75≤ξ≤2.0; ξ=(1.0-0.14[%C])×(1.005[%Si])×(1.0-0.056[%Mn])×(1.0+0.6[%P])×(1.0-0.36[%S])×(1 .0+0.30[%Cu])×(1.0+0.32[%Ni])×(1.0+0.70[%Ti])+21.28[%P]-3.5[%Ni]×[%P]+0.5[%Cr].
[0008] Furthermore, the chemical composition of the ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel satisfies the hardenability index of 1.50≤ф≤2.2; ф=2.4×[%C] 1 / 2 +1.4×[%Cr]+0.4×[%Ni]+2.1×[%Mo]+0.56×[%Mn]-1.68×[%Cu] 1 / 2 +1.386×[%Cu].
[0009] Furthermore, the following steps are included: using a converter for smelting, top and bottom combined blowing, and fully decarburizing and dephosphorizing to make the final carbon content 0.045% to 0.065% and the phosphorus content 0.060% ≤ P ≤ 0.080%; Through LF-RH refining, the harmful elements / impurities content is reduced and micro-alloying is performed; The casting is protected throughout the entire process, and heavy pressure reduction technology is used at the end of casting, with a reduction ratio of 12%~13%.
[0010] In a second aspect, the present invention provides an ultra-low yield ratio high-phosphorus atmospheric corrosion resistant steel produced by the above-mentioned preparation method.
[0011] Furthermore, the yield strength of the ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel is ≥350MPa, the tensile strength is ≥630MPa, the elongation after fracture is ≥20%, the yield ratio is ≤0.65, and the -40℃ KV2 is ≥47J.
[0012] Furthermore, the thickness of the ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel is ≤60mm.
[0013] Furthermore, the metallographic structure of the ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel is mainly uniform and fine ferrite + pearlite, and the ferrite grain size is greater than 10 levels.
[0014] Chemical composition is one of the important factors affecting the comprehensive performance of the product. The chemical composition of the present invention is restricted as follows.
[0015] C: The main solid solution strengthening element in steel, which can significantly improve the strength of steel plates, but a higher carbon content is not good for steel plate welding, toughness and plasticity. In order to effectively reduce segregation, improve microstructural uniformity, avoid galvanic corrosion caused by potential difference between different phases, improve the corrosion resistance of steel, and consider economic efficiency, the carbon content is limited to 0.05%~0.07%.
[0016] Si: Silicon is one of the effective deoxidizing and exothermic elements in the steelmaking process. It has a certain solid solution strengthening effect, is conducive to the formation of a dense rust layer, and can improve the atmospheric corrosion resistance of steel. However, too high a silicon content will reduce the surface quality, welding performance and low-temperature toughness of the steel. Therefore, the silicon content of the present invention is controlled at 0.10% to 0.20%.
[0017] Mn: Manganese has a strong solid solution strengthening effect, can significantly reduce the phase transition temperature of steel, refine the microstructure of steel, and is low in cost. It is an effective element for improving strength. In order to achieve sufficiently high tensile strength and obtain a low yield ratio, the content should not be less than 0.80%; but too high a content is likely to cause segregation of the ingot, forming a banded structure, reducing the weldability of the steel plate and the toughness of the welding heat affected zone, as well as the corrosion resistance. Therefore, the manganese content of the present invention is controlled at 1.20% to 1.35%.
[0018] P: Phosphorus can effectively improve the atmospheric corrosion resistance of steel. When phosphorus and copper are added to steel together, a better composite effect can be shown. However, too high a phosphorus content will significantly reduce the plasticity and low-temperature toughness of the steel, increase the cold brittleness of the steel, and deteriorate the welding performance.
[0019] S: Sulfur makes steel hot brittle, reduces the ductility and toughness of steel, and promotes the anisotropy of steel plates. Sulfide inclusions also significantly reduce the corrosion resistance of steel. The sulfur content in steel should be strictly controlled; the sulfur content of the present invention is controlled at ≤0.003%.
[0020] Al: Aluminum is one of the effective deoxidizing elements in the steelmaking process, which can effectively reduce the inclusion content in steel and refine the grains. However, if the content is too high, cracks are likely to occur on the surface of the ingot. The aluminum content of the present invention is controlled within a range of 0.010% to 0.040%.
[0021] Cr: Chromium is not only an element that improves the hardenability of steel, but also one of the effective elements to improve the weather resistance of steel. It has a significant effect on improving the passivation ability of steel and can promote the formation of a dense passivation film or protective rust layer on the steel surface. Its enrichment in the rust layer can effectively improve the selective permeability of the rust layer to corrosive media. However, too high a Cr content will increase production costs and reduce the toughness and weldability of steel.
[0022] Cu: Copper is one of the effective elements to improve the weather resistance of steel. It has a high electrochemical potential ratio, which can densify the rust on the surface of the steel plate and promote the formation of a stable rust layer. The addition of copper to steel is conducive to the formation of a dense, well-adhesive amorphous oxide (hydrocarbon oxide) protective layer on the surface of the steel, which has a significant corrosion resistance effect. In addition, copper and sulfur form insoluble sulfides, thereby offsetting the harmful effects of copper on the corrosion resistance of steel. However, when the copper content is too high, due to the low melting point of copper, which is lower than the heating temperature of the steel billet, the precipitated copper is in liquid and aggregates at the austenite grain boundary. When the precipitated copper content reaches a certain level, it is easy to produce cracks during heating or hot rolling.
[0023] Ni: Adding nickel to steel will significantly improve the corrosion resistance of the steel. At the same time, nickel and copper elements form a nickel-rich copper phase, which is retained in the outer oxide layer in a solid state, reducing the copper enrichment in the matrix and the chance of forming a liquid copper-rich phase, thereby avoiding hot brittle defects and reducing the sensitivity to hot cracks during casting, hot rolling and welding. In addition, nickel is also an indispensable alloying element for steel plates to obtain excellent low-temperature toughness, so the Ni / Cu content in steel is generally controlled to be ≥1 / 2. However, too much nickel will increase the adhesion of the oxide scale, and pressing it into the steel will form hot rolling defects on the surface. Moreover, nickel is a precious metal, and too high a nickel content will significantly increase the cost of steel alloys.
[0024] Ti: Titanium can produce strong precipitation strengthening and moderate grain refinement. The purpose of adding a trace amount of titanium to steel is to combine with nitrogen in the steel to generate highly stable titanium nitride particles, inhibit the growth of austenite grains in the HAZ area of welding and change the secondary phase transformation products, and improve the low-temperature toughness of high-energy input welding. The titanium content added to the steel must match the nitrogen content in the steel. When the titanium content is too little, the number of titanium nitride particles formed is insufficient to inhibit the growth of austenite grains in the HAZ and change the secondary phase transformation products to improve the low-temperature toughness of the HAZ in high-energy input welding; when the titanium content is too much, large-sized titanium nitride particles are precipitated during the solidification of the molten steel. Such large-sized particles not only cannot inhibit the growth of austenite grains in the HAZ, but will become the starting point for crack initiation.
[0025] The beneficial effects of the present invention are: The present invention adopts a low-cost micro-alloying design with a simple composition design. The weather resistance and comprehensive mechanical properties are improved by combining low carbon with trace elements such as P, Cu, Cr, Ni, etc., thereby reducing the amount of precious elements used. The weldability of the material is improved by a low-carbon equivalent design. The material is not dependent on a large reduction rate for rough rolling, but is produced by a controlled rolling process, so the production cycle is short and the cost is low, which is conducive to promotion and application.
[0026] The steel plate of the present invention has excellent strength-plasticity matching, welding performance, low yield ratio (≤0.65), weather resistance improved by more than 1.5 times, fatigue resistance, improved life and safety of structural parts, and is suitable for paint-free buildings and bridges, outdoor tower structural parts, and engineering machinery manufacturing fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0028] Figure 1 This is a metallographic picture of the 10 mm ultra-low yield ratio high-phosphorus atmospheric corrosion resistant steel prepared in Example 3. DETAILED DESCRIPTION
[0029] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0030] In the following examples, the marine atmospheric corrosion resistance index ξ is calculated according to the following formula: ξ=(1.0-0.14[%C])×(1.005[%Si])×(1.0-0.056[%Mn])×(1.0+0.6[%P])×(1.0-0.36[%S])×(1 .0+0.30[%Cu])×(1.0+0.32[%Ni])×(1.0+0.70[%Ti])+21.28[%P]-3.5[%Ni][%P]+0.5[%Cr].
[0031] The hardenability index ф is calculated according to the following formula: ф=2.4×[%C] 1 / 2 +1.4×[%Cr]+0.4×[%Ni]+2.1×[%Mo]+0.56×[%Mn]-1.68×[%Cu] 1 / 2 +1.386×[%Cu].
[0032] When the second stage of rolling begins, the surface temperature T2 of the rolled piece is calculated according to the following formula: T2=(T+1600 / H-1.8H)℃, Where T=870+11.2[%C]-1.8[%Si]+18[%Mn]+1.6[%Al]-1.2[%Cr], H is the thickness of the steel plate in mm.
[0033] Example 1 A 60mm ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel with the following chemical composition: C: 0.06%, Si: 0.16%, Mn: 1.32%, P: 0.068%, S: 0.001%, Als: 0.028%, Ni: 0.41%, Ti: 0.016%, the rest are Fe and unavoidable impurities. After calculation, the marine atmospheric corrosion resistance index ξ=1.53, and the hardenability index ф=1.49.
[0034] The preparation method is as follows: 1) The smelting converter adopts top and bottom combined blowing to fully decarburize and dephosphorize, with the end point carbon content of 0.03% and phosphorus content of 0.08%; LF is micro-alloyed, with the end point carbon of 0.040%, phosphorus content of 0.063%, and the micro-alloy content is added to the target value; RH vacuum reaches below 133pa, the pressure holding time is 13min, the pure degassing time is 11min, the soft blowing time is 12min, and the calming time after RH treatment is 33min.
[0035] 2) Heavy pressure reduction technology is used at the end of casting, and the reduction ratio is 12.6%.
[0036] 3) Slow cooling: After the billet is cut, it is placed in a slow cooling pit. The billet starts to cool slowly at 668°C and the billet exits the pit at 332°C.
[0037] 4) Heating: The billet charging temperature is 310℃, the billet exiting temperature is 1160℃, the time coefficient in the furnace is 10.2min / cm, and the temperature difference between the inside and outside of the billet is ≤10℃.
[0038] 5) Rolling: Two-stage rolling is adopted. The first stage rolling is carried out after the ingot is descaled. The surface temperature of the ingot at the first stage is 1067℃, and the surface temperature of the rolled piece at the second stage is T2=812℃. The steel plate is not water-cooled after rolling.
[0039] 6) Stack cooling: After rolling, the steel plate is quickly placed between 586℃ steel plates for stack cooling. The stack cooling time is 60 hours.
[0040] Example 2 A 30mm ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel with the following chemical composition: C: 0.05%, Si: 0.18%, Mn: 1.30%, P: 0.064%, S: 0.001%, Als: 0.026%, Cr: 0.62%, Ni: 0.4%, the rest are Fe and unavoidable impurities. After calculation, the marine atmospheric corrosion resistance index ξ=1.77, and the hardenability index ф=2.29.
[0041] The preparation method is as follows: 1) The smelting converter adopts top and bottom combined blowing to fully decarburize and dephosphorize, with the final carbon content of 0.03% and the phosphorus content of 0.085%; LF is micro-alloyed, with the final carbon content of 0.040% and the phosphorus content of 0.062%, and the micro-alloy content is added to the target value; the RH vacuum reaches below 133 Pa, the pressure holding time is 14 min, the pure degassing time is 10 min, the soft blowing time is 12 min, and the calming time after RH treatment is 35 min.
[0042] 2) Heavy pressure reduction technology is used at the end of casting, and the reduction ratio is 12.8%.
[0043] 3) Slow cooling: After the billet is cut, it is placed in a slow cooling pit. The billet starts to cool slowly at 670°C and the billet exits the pit at 326°C.
[0044] 4) Heating: The billet charging temperature is 308°C, the billet exiting temperature is 1162°C, the time coefficient in the furnace is 10.3min / cm, and the temperature difference between the inside and outside of the billet is ≤10°C.
[0045] 5) Rolling: Two-stage rolling is adopted. The first stage rolling is carried out after the ingot is descaled. The surface temperature of the ingot at the first stage is 1063℃, and the surface temperature of the rolled piece at the second stage is T2=892℃. The steel plate is not water-cooled after rolling.
[0046] 6) Stack cooling: After rolling, the steel plate is quickly placed between 576℃ steel plates for stack cooling. The stack cooling time is 53 hours.
[0047] Example 3 A 10mm ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel, the chemical composition is as follows: C: 0.06%, Si: 0.17%, Mn: 1.28%, P: 0.066%, S: 0.001%, Als: 0.023%, Cr: 0.68%, Cu: 0.39%, the rest are Fe and unavoidable impurities. After calculation, the marine atmospheric corrosion resistance index ξ=1.93, and the hardenability index ф=1.75.
[0048] The preparation method is as follows: 1) The smelting converter adopts top and bottom combined blowing to fully decarburize and dephosphorize, with the end point carbon content of 0.03% and phosphorus content of 0.083%; LF is micro-alloyed, with the end point carbon of 0.040%, phosphorus content of 0.063%, and the micro-alloy content is added to the target value; RH vacuum reaches below 133pa, the pressure holding time is 13min, the pure degassing time is 9min, the soft blowing time is 12min, and the calming time after RH treatment is 33min.
[0049] 2) Heavy pressure reduction technology is used at the end of casting, and the reduction ratio is 12.5%.
[0050] 3) Slow cooling: After the billet is cut, it is placed in a slow cooling pit. The billet starts to cool slowly at 676°C and the billet exits the pit at 328°C.
[0051] 4) Heating: The charging temperature of the billet is 311°C, the discharging temperature of the billet is 1168°C, the time coefficient in the furnace is 10.7min / cm, and the temperature difference between the inside and outside of the billet is ≤10°C.
[0052] 5) Rolling: Two-stage rolling is adopted. The first stage rolling is carried out after the ingot is descaled. The surface temperature of the ingot at the beginning of the first stage rolling is 1078℃. The surface temperature of the rolled piece at the beginning of the second stage rolling is T2=1035℃. The steel plate is not water-cooled after rolling.
[0053] 6) Stack cooling: After rolling, the steel plate is quickly placed between 596℃ steel plates for stack cooling. The stack cooling time is 55 hours.
[0054] The steel plates of Examples 1 to 3 were observed, and the metallographic structures of the steel plates were fine and uniform, mainly ferrite + pearlite, wherein the grain size of the ferrite reached a level of >10.
[0055] The comprehensive properties of the steel plates of Examples 1 to 3 were tested, and the results are shown in Table 1 below.
[0056] Table 1 Tensile properties and low temperature toughness of the steel plates of the present invention
[0057] As shown in Table 1, the steel plate prepared by the method of the present invention has a lower yield strength ratio. Figure 1 It can be seen that the steel plate prepared by the method of the present invention has fine grains and uniform structure. It can be concluded that the method of the present invention can greatly enhance the safety and anti-seismic and anti-fatigue capabilities of structural parts. Although the phosphorus content is high, the excellent structure allows the steel plate to still have good toughness at -40°C.
[0058] The electrochemical corrosion potential of the steel plates of Examples 1 to 3 was measured using a three-electrode system: the working electrodes were 10×10 mm 2 The bare plate electrode and the rusted electrode prepared after 30 dry-wet alternating cycles of corrosion, the reference electrode is a saturated calomel electrode (SCE), and the auxiliary electrode is a 9cm 2 The platinum sheet was used, and the working electrode and the reference electrode were connected by a salt bridge. The working temperature was room temperature 25°C, and all potential values were relative to the potential of the saturated calomel electrode. The polarization curve was scanned by Solartron1287 dynamic potential, with a scanning potential range of ±0.2V vs.Ecorr (relative to the self-corrosion potential) and a scanning speed of 0.1667mV / s. The experiment was carried out at room temperature. The self-corrosion potential after electrochemical determination is shown in Table 2 below.
[0059] Table 2 Self-corrosion potential of steel plates according to the present invention
[0060] It can be seen from the data in Table 2 that the self-corrosion potential of the steel plate produced by the method of the present invention is lower than that of the American standard weathering steel Corten-A, indicating that the corrosion resistance of the ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel provided by the present invention is higher than that of the American standard weathering steel Corten-A.
[0061] The steel plates of Examples 1 to 3 were processed into standard specimens according to "TB / T 2375-1993 Test Method for Periodic Immersion Corrosion of Weathering Steel for Railway Use" and compared with Corten-A steel. A 72-hour periodic immersion test was performed. The test results are shown in Table 3.
[0062] Table 3 Cyclic infiltration test results of steel plates according to the present invention
[0063] It can be seen from the data in Table 3 that the steel plate produced by the present method has a weight loss much lower than that of the American standard weathering steel Corten-A under the same corrosion conditions, indicating that the corrosion resistance of the ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel provided by the present invention is higher than that of the American standard weathering steel Corten-A.
[0064] Although the present invention has been described in detail with reference to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention.
Claims
1. A method for preparing ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel, characterized in that: The chemical composition and weight percentage of ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel are C: 0.05%~0.07%, Si: 0.10%~0.20%, Mn: 1.20%~1.35%, 0.060%≤P≤0.080%, S≤0.003%, Als: 0.010%~0.040%, Cr≤0.80%, Cu≤0.50%, Ni≤0.50%, Ti≤0.020%, and the balance is Fe and unavoidable impurities; The preparation method comprises at least the following steps: Put the cut ingot into the slow cooling pit, the starting slow cooling temperature of the ingot is ≥500℃, and the ending slow cooling temperature is not less than 300℃; Heat the slowly cooled ingot, control the ingot out-of-furnace temperature to be 1140~1170℃, and the furnace time coefficient to be 10~11min / cm; Two-stage rolling is adopted. The first stage rolling is carried out after the billet is descaled. When the second stage rolling starts, the surface temperature of the rolled piece is T2=(T+1600 / H-1.8H)℃, where T=870+11.2[%C]-1.8[%Si]+18[%Mn]+1.6[%Al]-1.2[%Cr], H is the thickness of the steel plate in mm, and the steel plate is not water-cooled after rolling; After rolling, the steel plate is placed in a pile cooling room at 500~600℃ for no less than 48 hours.
2. The preparation method according to claim 1, characterized in that The chemical composition of ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel meets the marine atmospheric corrosion resistance index of 1.50≤ξ≤2.0; ξ=(1.0-0.14[%C])×(1.005[%Si])×(1.0-0.056[%Mn])×(1.0+0.6[%P])×(1.0-0.36[%S])×(1 .0+0.30[%Cu])×(1.0+0.32[%Ni])×(1.0+0.70[%Ti])+21.28[%P]-3.5[%Ni]×[%P]+0.5[%Cr].
3. The preparation method according to claim 1, characterized in that: The chemical composition of ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel meets the hardenability index of 1.40≤ф≤2.4; ф=2.4×[%C] 1 / 2 +1.4×[%Cr]+0.4×[%Ni]+2.1×[%Mo]+0.56×[%Mn]-1.68×[%Cu] 1 / 2 +1.386×[%Cu]。 4. The preparation method according to claim 1, characterized in that: The process also includes the following steps: using a converter for smelting, top and bottom combined blowing, and fully decarburizing and dephosphorizing to make the final carbon content 0.045% to 0.065% and the phosphorus content 0.060% ≤ P ≤ 0.080%; Through LF-RH refining, the harmful elements / impurities content is reduced and micro-alloying is performed; The casting is protected throughout the entire process, and heavy pressure reduction technology is used at the end of casting, with a reduction ratio of 12%~13%.
5. An ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel produced by the preparation method according to any one of claims 1 to 4.
6. The ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel according to claim 5, characterized in that: The yield strength of ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel is ≥350MPa, tensile strength ≥630MPa, elongation after fracture ≥20%, yield ratio ≤0.65, -40℃ KV2 ≥47J.
7. The ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel according to claim 5, characterized in that: The thickness of ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel is ≤60mm.
8. The ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel according to claim 5, characterized in that: The metallographic structure of ultra-low yield ratio high phosphorus atmospheric corrosion resistant steel is mainly ferrite + pearlite, and the ferrite grain size is greater than 10 levels.
Citation Information
Patent Citations
Low-yield-ratio cold-rolled weathering-resistant steel and production method thereof
CN106893950A
345MPa-grade low-yield-ratio weather-resistant steel and preparation method thereof
CN109234635A
440-MPa-grade high-phosphorus and high-chrome weathering steel and preparation method and application thereof
CN111926254A
Steel with low yield ratio and high toughness and preparation method thereof
CN114134414A
Easily-welded coating-free 420MPa-grade marine atmosphere corrosion-resistant steel plate and manufacturing method thereof
CN117265411A