A kind of blue IZO powder and preparation method thereof

Through spray granulation and heat treatment technology, blue IZO powder rich in oxygen vacancies was prepared, which solved the problem of insufficient conductivity and device performance of IZO materials in the existing technology, and significantly improved the conductivity and device performance.

CN116216770BActive Publication Date: 2024-10-29XIANDAO THIN FILM MATERIALS GUANGDONG CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211615697.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-15
Publication Date
2024-10-29
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

It is difficult to effectively prepare IZO materials with rich oxygen vacancies in the existing technology, resulting in insufficient conductivity, transmittance and efficiency of optoelectronic devices, and stability of electrochemical devices.

Method used

Using the spray granulation method of materials such as indium oxide, zinc oxide, and tin dioxide, combined with heat treatment and washing steps, blue IZO powder with rich oxygen vacancies was prepared. By adjusting the spray granulation temperature, drying temperature, and reducing agent addition quantity and heat treatment conditions to optimize the oxygen vacancy concentration.

Benefits of technology

It improves the conductivity of IZO materials, enhances the transmittance and efficiency of optoelectronic devices, and improves the stability of electrochemical devices.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present application relates to the field of semiconductor technology, and discloses a method for preparing blue IZO powder, comprising the following steps: step 1: mixing indium oxide, zinc oxide, tin dioxide, a dispersant, and pure water to obtain slurry 1; step 2: spraying and granulating the slurry 1 obtained in step 1 to obtain yellow IZO precursor powder; step 3: adding a reducing agent to the yellow IZO precursor powder obtained in step 2, adding it to an autoclave after shearing with an emulsifying shearing machine, and separating the solid and liquid after heat treatment to obtain a blue precipitate; step 4: washing the blue precipitate obtained in step 3 with pure water, drying it, and obtaining a blue IZO powder. The blue IZO powder prepared by the method has a higher oxygen vacancy concentration, thereby improving its carrier concentration and conductivity. In addition, a blue IZO powder is also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor production technology, and in particular to a blue IZO powder and a preparation method thereof. Background Art

[0002] Semiconductors refer to materials with electrical conductivity between conductors and insulators at room temperature. Semiconductors are widely used in radios, televisions, and temperature measuring equipment. In recent years, the research momentum of amorphous semiconductors has gradually increased, mainly because of the following characteristics of amorphous semiconductors:

[0003] Structurally, the constituent atoms of amorphous semiconductors have no long-range order, but because the bonding force between atoms is very similar to that of crystals, they usually still maintain short-range order within the range of several lattice constants, which is the characteristic of amorphous materials, long-range disorder and short-range order. At the same time, for most amorphous semiconductors, their constituent atoms are bound together by covalent bonds to form a continuous covalent bond network. All valence electrons are bound in the bonds and satisfy the (8-N) rule of the maximum number of built-in electrons. This is usually called bond saturation.

[0004] Chinese Patent No. 201410818288.3 discloses a P-type metal oxide semiconductor material and a method for manufacturing the same. The P-type metal oxide semiconductor material has In (1-a) Ga (1-b) Zn (1+a+b) O 4 , wherein 0≤a≤0.1, 0≤b≤0.1, and 0<a+b≤0.16, and the p-type metal oxide semiconductor material has a hole carrier concentration between 1×10 11 cm to 5×10 11 cm*.

[0005] At the same time, the manufacturing method of the P-type metal oxide semiconductor material is: mixing an indium salt, a gallium salt, and a zinc salt in a solvent to obtain a mixture; adding a chelating agent to the mixture to form a metal zirconium compound including steel, arsenic, and zinc; and subjecting the metal zirconium compound to a heat treatment to form a P-type metal oxide semiconductor material.

[0006] This scheme successfully prepared a new indium gallium zinc oxide-based P-type transparent semiconductor material through the above method, solving the problem that P-type semiconductor materials have relatively unstable characteristics, poor reproducibility and rare species during development.

[0007] Chinese patent 201911328118.6 discloses a deep blue tungsten oxide nanowire and a preparation method thereof, comprising the steps of coating liquid metal on the surface of a flexible substrate to form a flexible substrate containing a liquid metal coating, and then subjecting the flexible substrate to a hydrothermal reaction with a tungsten salt reagent.

[0008] This method is used to prepare a deep blue tungsten oxide nanowire, which contains abundant oxygen vacancies and is suitable for optoelectronic devices and electrochemical devices.

[0009] The problem that this program needs to solve: How to develop a method for preparing IZO materials with abundant oxygen vacancies. Summary of the invention

[0010] The purpose of the present invention is to provide an IZO material and a preparation method thereof. The IZO prepared by the method has abundant oxygen vacancies. At the same time, the abundant oxygen vacancies increase the concentration of carriers inside the IZO, thereby improving the conductivity of the IZO material. At the same time, as the oxygen vacancy concentration increases, the transmittance and efficiency of the optoelectronic device made therefrom are improved accordingly, and at the same time, it has a positive effect on the stability of the electrochemical device.

[0011] A method for preparing blue IZO powder comprises the following steps:

[0012] Step 1: Mix indium oxide, zinc oxide, tin dioxide, a dispersant and pure water to obtain slurry 1;

[0013] Step 2: spray granulate the slurry 1 obtained in step 1 to obtain yellow IZO precursor powder;

[0014] Step 3: Add a reducing agent to the yellow IZO precursor powder obtained in step 2, add it to an autoclave after shearing with an emulsifying shearing machine, separate the solid and liquid after heat treatment, and obtain a blue precipitate;

[0015] Step 4: Wash the blue precipitate obtained in step 3 with pure water, dry it, and obtain blue IZO powder;

[0016] In practical applications, preferably, the temperature of spray granulation is 90-110°C; and the drying temperature is 100-120°C.

[0017] More preferably, the temperature of spray granulation includes but is not limited to 90°C, 95°C, 100°C, 105°C, 110°C; the drying temperature includes but is not limited to 100°C, 105°C, 110°C, 115°C, 120°C;

[0018] It should be noted and understood that the present application does not impose too many restrictions on the time and temperature of drying, the time and temperature of spray granulation, and those skilled in the art may make certain modifications to the temperature and time of spray granulation and drying according to actual conditions. The spray granulation temperature and drying temperature mentioned in the present application are the preferred spray granulation temperature and drying temperature with higher production efficiency in the embodiments, which may fluctuate due to different reaction containers, environments and other factors, but this fluctuation has no essential effect on the problem to be solved by the present application.

[0019] Preferably, the mass ratio of indium oxide, zinc oxide and tin dioxide is 85-95:5-15:1-5;

[0020] More preferably, the mass ratio of indium oxide, zinc oxide and tin dioxide includes but is not limited to 85:5:1, 90:5:1, 95:5:1, 85:10:1, 90:10:1, 95:10:1, 85:15:1, 90:15:1, 95:15:1, 85:5:5, 90:5:5, 95:5:5, 85:10:5, 90:10:5, 95:10:5, 85:15:5, 90:15:5 and 95:15:5.

[0021] The dispersant accounts for 1-10% of the total mass of the added indium oxide powder, zinc oxide powder and tin dioxide powder;

[0022] The average particle size of the indium oxide is 120-250 nm;

[0023] The average particle size of the zinc oxide is 120-250 nm;

[0024] The average particle size of the tin dioxide is 120-250nm;

[0025] The solid content in the slurry 1 is between 50% and 70%.

[0026] More preferably, the dispersant accounts for 2%-8% of the total mass of the added indium oxide powder, zinc oxide and tin dioxide powder. In practical applications, the added amount of the dispersant includes but is not limited to 2%, 3%, 4%, 5%, 6%, 7%, 8% of the total mass of the indium oxide powder, zinc oxide and tin dioxide powder;

[0027] The average particle size of the indium oxide includes but is not limited to 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 210nm, 220nm, 230nm, 240nm, 250nm;

[0028] The average particle size of the zinc oxide includes but is not limited to 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 210nm, 220nm, 230nm, 240nm, 250nm;

[0029] The average particle size of the tin dioxide includes but is not limited to 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, 210 nm, 220 nm, 230 nm, 240 nm, and 250 nm.

[0030] The solid content of the slurry 1 is between 55% and 65%.

[0031] Preferably, the dispersant in step 1 is selected from one or more of polyvinyl pyrrolidone, polycarboxylic acid compounds, and polyvinyl salts;

[0032] The polycarboxylic acid compound is selected from at least one of maleic acid sodium acrylate and acrylic acid copolymer;

[0033] The polyvinyl salt is selected from at least one of polyoxyethylene alkylphenol ether and polyethyl acetate.

[0034] Preferably, the reducing agent in step 3 is selected from one or more of aniline, oxalic acid, ethanol, and ethylene glycol;

[0035] The reducing agent accounts for 40-60% of the mass of the yellow IZO precursor powder.

[0036] More preferably, the reducing agent includes but is not limited to 40%, 45%, 50%, 55%, 60% of the mass of the yellow IZO precursor powder.

[0037] Preferably, the heat treatment in step 3 is performed at a temperature of 280°C-300°C and for a time of 460-500 minutes.

[0038] More preferably, the temperature of the heat treatment in step 3 includes but is not limited to 280°C, 285°C, 290°C, 295°C, 300°C;

[0039] The heat treatment time includes but is not limited to 460 minutes, 465 minutes, 470 minutes, 475 minutes, and 480 minutes.

[0040] Preferably, in step 1, a disperser is used to mix indium oxide, zinc oxide, tin dioxide, a dispersant and pure water, and the rotation speed of the disperser is 400-600 r / min.

[0041] More preferably, in practical applications, the speed of the disperser is 450-550 r / min.

[0042] In addition, a blue IZO powder is also disclosed, which is prepared by the above-mentioned preparation method of the blue IZO powder.

[0043] Preferably, the particle size of the blue IZO powder is 8 μm-12 μm.

[0044] Preferably, the specific surface area of ​​the blue IZO powder is 11 m 2 / g-15m 2 / g.

[0045] The beneficial effects of this application are:

[0046] The present application discloses a method for preparing an IZO powder. The IZO prepared by the method has abundant oxygen vacancies. The abundant oxygen vacancies increase the concentration of carriers inside the IZO, thereby improving the conductivity of the IZO material. At the same time, as the concentration of oxygen vacancies increases, the transmittance and efficiency of the optoelectronic device made therefrom increase accordingly, and it has a positive effect on the stability of the electrochemical device. DETAILED DESCRIPTION

[0047] The present application will be described clearly and completely below in conjunction with the examples of the present application. In the description of the present application, it should be noted that if the specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0048] Example 1

[0049] Step 1: Add 17.0 kg of indium oxide powder, 3.0 kg of zinc oxide powder, 0.2 kg of tin dioxide powder, 0.404 kg of polyvinyl pyrrolidone and 13.74 kg of pure water into a mixing barrel, and then disperse for 60 minutes to obtain slurry 1. The speed of the disperser is 500 r / min, the average particle size of indium oxide is 200 nm, the average particle size of zinc oxide is 200 nm, and the average particle size of tin dioxide is 200 nm.

[0050] Step 2: spray granulate the slurry 1 obtained in step 1 to obtain yellow IZO precursor powder. The spray granulation temperature is 100°C;

[0051] Step 3: Take 2.0 kg of the yellow IZO precursor powder obtained in step 2 and add 1.0 kg of aniline thereto, add it into an autoclave after emulsification and shearing, and heat treat it at 290°C for 480 min, and then separate the solid and liquid to obtain a blue precipitate;

[0052] Step 4: Wash the blue precipitate obtained in step 3 with pure water, and then dry it at a temperature of 100° C. for 3 hours to obtain the blue IZO powder.

[0053] Example 2

[0054] It is basically the same as Example 1, except that the added amount of indium oxide powder is 18 kg, the added amount of zinc oxide powder is 2 kg, and the added amount of tin dioxide powder is 0.4 kg.

[0055] Example 3

[0056] It is basically the same as Example 1, except that in step 1, the amount of indium oxide powder added is 19 kg, the amount of zinc oxide powder added is 1 kg, the amount of tin dioxide powder added is 1 kg, the average particle size of indium oxide is 120 nm, the average particle size of zinc oxide is 200 nm, and the average particle size of tin dioxide is 250 nm.

[0057] Example 4

[0058] The method is basically the same as Example 1, except that the dispersant is polyethyl acetate, the amount added is 1.414 kg, the speed of the disperser is 400 r / min, and the dispersion time is 80 minutes;

[0059] The temperature of the spray granulation was 90°C.

[0060] Example 5

[0061] The method is basically the same as Example 1, except that the dispersant is sodium maleic acid acrylate, the amount added is 1.616 kg, the speed of the disperser is 500 r / min, and the dispersion time is 40 minutes;

[0062] The temperature of the spray granulation was 110°C.

[0063] Example 6

[0064] The method is basically the same as Example 1, except that the reducing agent in step 3 is ethylene glycol, and the amount added is 0.8 kg;

[0065] The heat treatment temperature is 280° C., and the heat treatment time is 460 minutes.

[0066] Example 7

[0067] The method is basically the same as Example 1, except that the reducing agent in step 3 is ethanol, and the amount added is 1.2 kg;

[0068] The heat treatment temperature is 300° C., and the heat treatment time is 460 minutes.

[0069] Comparative Example 1

[0070] It is basically the same as Example 1, except that no dispersant is added.

[0071] Comparative Example 2

[0072] The process is substantially the same as Example 1, except that 0.2 kg of aniline is added in step 3.

[0073] Comparative Example 3

[0074] The process is substantially the same as Example 1, except that 2 kg of aniline is added in step 3.

[0075] Comparative Example 4

[0076] It is basically the same as Example 1, except that the heat treatment temperature is 200°C.

[0077] Comparative Example 5

[0078] It is basically the same as Example 1, except that the heat treatment temperature is 400°C.

[0079] Comparative Example 6

[0080] The method is basically the same as Example 1, except that tin dioxide is not added.

[0081] Performance Testing:

[0082] Particle size testing method: laser particle size analyzer;

[0083] Specific surface area test method: nitrogen adsorption tester;

[0084] Oxygen vacancy concentration test method: XPS test (X-ray photoelectron spectroscopy technology).

[0085] Table 1: Blue IZO performance test results

[0086] Particle size (μm) <![CDATA[Specific surface area (m 2 / g)]]> <![CDATA[Oxygen vacancy concentration (cm -3 )]]> Example 1 9.54 13.46 <![CDATA[6.47×10 19 ]]> Example 2 11.36 11.64 <![CDATA[8.76×10 19 ]]> Example 3 10.58 12.68 <![CDATA[6.78×10 19 ]]> Example 4 11.09 11.71 <![CDATA[7.87×10 19 ]]> Example 5 9.36 13.08 <![CDATA[6.24×10 19 ]]> Example 6 10.86 12.64 <![CDATA[6.14×10 19 ]]> Example 7 11.30 11.91 <![CDATA[4.87×10 19 ]]> Comparative Example 1 16.87 10.01 <![CDATA[3.87×10 16 ]]> Comparative Example 2 15.97 10.86 <![CDATA[8.74×10 15 <!-- 4 -->]]> Comparative Example 3 9.34 13.28 <![CDATA[5.34×10 15 ]]> Comparative Example 4 9.64 13.39 <![CDATA[8.14×10 16 ]]> Comparative Example 5 12.81 10.11 <![CDATA[3.41×10 14 ]]> Comparative Example 6 8.69 10.82 <![CDATA[7.68×10 14 ]]>

[0087] Result analysis:

[0088] 1. It can be seen from Examples 1-3 that when the mass ratio of indium oxide, zinc oxide, and tin dioxide is 90:10:2, the oxidation vacancy concentration is significantly higher than that of Examples 1 and 3. At the same time, compared with Example 2, the proportion of zinc oxide in Example 1 is higher; at the same time, the proportion of indium oxide and tin dioxide in Example 3 is higher, and the proportion of zinc oxide is smaller; therefore, we speculate that the reason why the oxygen vacancy concentration of Examples 1 and 3 is significantly different from that of Example 2 may be that when the mass ratio of indium oxide, zinc oxide, and tin dioxide is 90:10:2, the three interact with each other and increase the number of defects in the indium zinc oxide powder, so that the oxygen vacancy concentration is greatly improved.

[0089] 2. It can be seen from Examples 1 and 4-5 that when the amount of dispersant added is 7% of the total mass of indium oxide powder, zinc oxide powder and tin dioxide powder, the oxygen vacancy concentration is significantly higher than that of Examples 1 and 5, but the amount of dispersant used in Example 5 is greater than that in Example 4. Generally, adding more dispersant is beneficial to improving the dispersion effect. At the same time, compared with Examples 1 and 5, although the rotation speed of Example 4 is not as good as that of Examples 1 and 5, its dispersion time is longer. Therefore, we speculate that, relative to the blue IZO preparation method, long-term continuous stirring is relative to adding more dispersant, and its dispersion effect is better.

[0090] 3. It can be seen from Example 1 and Examples 6-7 that while the heat treatment temperature and time of Example 1, Example 6, and Example 7 are relatively small, their oxygen vacancy concentrations have such a large difference. The difference between the three is that the amount of reducing agent added is 50%, 40%, and 60% of the mass of the yellow indium zinc oxide precursor, respectively, and the oxygen vacancy concentration first increases and then decreases with the increase in the amount of reducing agent added. Therefore, we speculate that the increase in the amount of reducing agent added leads to a decrease in the activation energy of the indium zinc oxide precursor, which in turn causes an increase in the oxygen vacancy concentration. When the concentration of the reducing agent is further increased, part of the indium zinc oxide precursor particles are wrapped by the reducing agent, resulting in part of the indium zinc oxide precursor being unable to react, thereby causing a decrease in the oxygen vacancy concentration.

[0091] 4. It can be seen from Example 1 and Comparative Example 1 that when no dispersant is added, the mixing degree of indium oxide powder, zinc oxide powder and tin dioxide powder is too low, resulting in a large amount of agglomeration and thus a significant reduction in the oxygen vacancy concentration.

[0092] 5. It can be seen from Example 1 and Comparative Examples 2-3 that when the amount of reducing agent added is 10% and 100% of the mass of the yellow indium zinc oxide precursor, the oxygen vacancy concentration of indium zinc oxide is greatly reduced. We speculate that when the reducing agent is too little, part of the indium zinc oxide cannot produce defects; when the reducing agent is too much, part of the indium zinc oxide particles are surrounded by the reducing agent and cannot react.

[0093] 6. It can be seen from Example 1 and Comparative Examples 4-5 that when the heat treatment temperature is too high or too low, the oxygen vacancy concentration of indium zinc oxide is greatly reduced. We speculate that when the temperature is too high, part of the reducing agent fails to function, resulting in too low an oxygen vacancy concentration; when the temperature is too low, insufficient energy is provided to generate oxygen vacancies, resulting in too low an oxygen vacancy concentration.

[0094] 7. It can be seen from Example 1 and Comparative Example 6 that when tin dioxide is not added to the raw material, the oxygen vacancy concentration of indium zinc oxide is greatly reduced. We speculate that the lack of tin dioxide may cause indium zinc oxide to have a higher activation energy, and higher energy is required to generate oxygen vacancies.

[0095] 8. It can be seen from Examples 1-8 and Comparative Examples 1-6 that there is a certain gap between the examples and the comparative examples in terms of particle size and specific surface area, but generally speaking the gap is not large. However, it should be noted that if the particle size of the IZO powder is too small during the production process, agglomeration may occur. When the particle size is between 8 and 12 μm, the agglomeration phenomenon will be reduced to a certain extent. However, at the same time, as the particle size continues to increase, the degree of IZO crystallization increases, the number of defects decreases, and oxygen vacancies are adversely affected. In addition, the specific surface area in the present application is greatly affected by the particle size and the defect concentration itself.

Claims

1. A method for preparing blue IZO powder, characterized in that: The following steps are involved: Step 1: Mix indium oxide, zinc oxide, tin dioxide, a dispersant and pure water to obtain slurry 1; Step 2: spray granulate the slurry 1 obtained in step 1 to obtain yellow IZO precursor powder; Step 3: Add a reducing agent to the yellow IZO precursor powder obtained in step 2, add it to an autoclave after shearing with an emulsifying shearing machine, separate the solid and liquid after heat treatment, and obtain a blue precipitate; Step 4: Wash the blue precipitate obtained in step 3 with pure water, dry it, and obtain blue IZO powder; The reducing agent in step 3 is selected from one or more of aniline, oxalic acid, ethanol, and ethylene glycol; The reducing agent accounts for 40-60% of the mass of the yellow IZO precursor powder; The heat treatment temperature in step 3 is 280°C-300°C, and the heat treatment time is 460-500 minutes; The mass ratio of indium oxide, zinc oxide and tin dioxide is 85-95:5-15:1-5.

2. The method for preparing blue IZO powder according to claim 1, characterized in that: In step 1, the dispersant accounts for 1-10% of the total mass of the added indium oxide powder, zinc oxide powder, and tin dioxide powder; The average particle size of the indium oxide is 120-250 nm; The average particle size of the zinc oxide is 120-250 nm; The average particle size of the tin dioxide is 120-250nm; The solid content in the slurry 1 is between 50% and 70%.

3. The method for preparing blue IZO powder according to claim 1, characterized in that: The dispersant in step 1 is selected from at least one of polyvinyl pyrrolidone, sodium maleic acid acrylate, acrylic acid copolymer, polyoxyethylene alkylphenol ether, and polyethyl acetate.

4. The method for preparing blue IZO powder according to claim 1, characterized in that: The temperature of spray granulation is 90-110°C, the temperature of drying is 100-120°C, and the drying time is 1-5 hours.

5. The method for preparing blue IZO powder according to claim 1, characterized in that: In step 1, indium oxide, zinc oxide, tin dioxide, a dispersant and pure water are mixed using a disperser, the speed of the disperser is 400-600 r / min, and the dispersion time of the disperser is 40-80 minutes.

6. A blue IZO powder, characterized in that: The blue IZO powder is prepared by the preparation method of any one of claims 1 to 5.

7. The blue IZO powder according to claim 6, characterized in that: Its particle size is 8-12μm.

8. The blue IZO powder according to claim 6, characterized in that: Its specific surface area is 11-15m 2 / g.

Citation Information

Patent Citations

  • P-type metal oxide semiconductor material and method for fabricating the same

    CN104810387A

  • Dark blue tungsten oxide nanowire and preparation method thereof

    CN113003607A

  • Method for preparing novel conductive indium tin zinc oxide thin film

    CN103572230A

  • Preparation method of blue nanometer tin indium oxide powder

    CN103771499A

  • Method for preparing ITO (Indium Tin Oxide) granulation powder by mixing method

    CN111138202A