A strontium titanate-based microwave dielectric ceramic material and a preparation method thereof
The sintering characteristics and dielectric properties of Sr2TiO4 microwave dielectric ceramics are optimized through ionic substitution, and the problem of poor temperature stability is solved, and the preparation of strontium titanate-based microwave dielectric ceramic materials with high Q and temperature stability is realized. , suitable for communications.
Patent Information
- Application Number
- CN202310228034.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-03-10
AI Technical Summary
The poor temperature stability of existing Sr2TiO4 microwave dielectric ceramics limits its application in the field of communications.
Sr2-xLaxTi1-xO4, a strontium titanate-based microwave dielectric ceramic material, was prepared by ionic substitution, and its sintering characteristics and microwave dielectric properties were optimized. The specific steps include ball milling, drying, prefiring, granulation, and glue removal. and sintering, the sintering temperature is between 1550°C and 1575°C to form a microwave dielectric ceramic with improved temperature stability.
It significantly improves the temperature stability, dielectric constant and quality factor of microwave dielectric ceramics, reduces the resonant frequency temperature coefficient, and optimizes the dielectric performance, and is suitable for mass production in the communication field.
Smart Images

Figure CN116217225B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of microwave dielectric ceramic materials, and in particular relates to a strontium titanate-based microwave dielectric ceramic and a preparation method thereof. Background Art
[0002] At present, microwave dielectric ceramic systems used in microwave communications such as mobile communications and satellite communications have problems such as high prices, harsh preparation conditions, and large dielectric losses. With the widespread development of modern electronic devices and wireless communication systems, the scale and consumption demand of microwave dielectric ceramics in China are growing rapidly. Therefore, it is necessary to develop a series of microwave dielectric ceramic materials with suitable dielectric constants, low dielectric losses, near-zero resonant frequency temperature coefficients, and suitable sintering temperatures.
[0003] Among them, microwave dielectric ceramics with K2NiF4 structure have attracted more and more attention due to their ultra-low dielectric loss. Among microwave dielectric ceramics with this structure, Sr2TiO4 ceramics have attracted extensive attention from researchers due to their good microwave dielectric properties, but their high resonant frequency temperature coefficient (~142 ppm / ℃) limits their application. Summary of the invention
[0004] In order to solve the problem of poor temperature stability of Sr2TiO4 microwave dielectric ceramics in the prior art, the present invention focuses on a method of forming a solid solution through ion substitution, improves its sintering characteristics and microwave dielectric properties, and ultimately finds a microwave dielectric ceramic material with high Q and good temperature stability that can be applied to the communication field and its preparation method.
[0005] The strontium titanate-based microwave dielectric ceramic material of the present invention has a chemical expression of Sr 2-x La x Ti 1-x Al x O4, where 0.2≤ x ≤0.8.
[0006] Better, 0.2 ≤ x ≤0.8, preferably 0.4.
[0007] Preferably, the x =0.4, the dielectric properties of strontium titanate-based microwave dielectric ceramics are ε r =22.5, Q×f =75464 GHz, τ f =-7.3 ppm / ℃.
[0008] The strontium titanate-based microwave dielectric ceramic material of the present invention can be obtained by the following preparation method, which specifically comprises the following steps:
[0009] (1) SrCO3, La2O3, Al2O3 and TiO2 are used as raw materials and the raw materials are ball-milled once using a planetary ball mill according to the chemical expression ratio.
[0010] (2) The slurry obtained after step (1) is dried, ground, sieved and pre-calcined, and the pre-calcined powder is subjected to secondary ball milling.
[0011] (3) The slurry obtained after step (2) is dried, passed through a 60-mesh sieve, granulated, passed through a 40-mesh sieve, tableted, and debinded to obtain a ceramic green body.
[0012] (4) Sintering the green body obtained in step (3) at 1550°C-1575°C to obtain microwave dielectric ceramics.
[0013] Preferably, in the step (1), the La2O3 needs to be pre-treated by calcining at 900°C for 2 hours before weighing.
[0014] Preferably, in step (1), the primary ball milling medium is anhydrous ethanol, the ball milling bead material is ZrO2, the ball milling jar is a nylon jar, and the ball milling time is 4 hours.
[0015] Preferably, in step (2), a 60-mesh standard sieve is used for sieving, and the pre-burning temperature is 1400°C, which is increased to 1400°C at a heating rate of 5°C per minute, and pre-burned at 1400°C for 4 hours, and then naturally cooled to room temperature.
[0016] Preferably, in step (2), the secondary ball milling medium is anhydrous ethanol, the ball milling bead material is ZrO2, the ball milling jar is a nylon jar, and the ball milling time is 8 hours.
[0017] Preferably, in the step (3), the granulation uses a PVA solution with a concentration of 10 wt% as a binder, the sieving before and after the granulation uses standard sieves of 60 mesh and 40 mesh respectively, and the tableting is dry-pressed using a stainless steel mold; the debinding is to place the ceramic green body in a muffle furnace and calcine it at 550°C for 5 hours, in order to discharge the PVA component used for bonding.
[0018] Preferably, in step (4), the sintering process is to first increase the temperature to 1100°C at a heating rate of 5°C per minute, then increase the temperature to 1550°C~1575°C at a heating rate of 3°C per minute, and keep the temperature for 4 hours; after the insulation is completed, the temperature is reduced to 1100°C at a cooling rate of 2°C per minute, and then naturally cooled to room temperature.
[0019] The beneficial effects of the present invention are:
[0020] The present invention improves the temperature stability of Sr2TiO4 microwave dielectric ceramics by forming a solid solution, and the dielectric constant thereof is (18.2-27.1), the quality factor is (59501-102136 GHz), and the resonant frequency temperature coefficient is -38.2-16.7 ppm / ℃. Preferably, the x =0.4, the dielectric properties of strontium titanate-based microwave dielectric ceramics are ε r =22.5, Q×f =75464 GHz, τ f =-7.3 ppm / ℃. The preparation process is simple and effective, the experiment has strong repeatability, can be mass-produced, and can be applied to the communication field. The above characteristics make the present invention have important industrial application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The X-ray diffraction patterns of Comparative Example 1 and Examples 1-4 of the present invention are shown.
[0022] Figure 2 This is the SEM image of Comparative Example 1 of the present invention.
[0023] Figure 3 This is the SEM image of Example 2. Implementation
[0024] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0025] Embodiment 1:
[0026] Sr 1.8 La 0.2 Ti 0.8 Al 0.2 O4 microwave dielectric ceramic and preparation method thereof, the preparation process comprises the following steps:
[0027] (1) Ingredient weighing: According to Sr 2-x La x Ti 1-x Al x O4( x =0.2) are weighed out of calcined SrCO3, La2O3, Al2O3 and TiO2 powders.
[0028] (2) Primary ball milling: The weighed raw materials were transferred into a nylon ball mill jar, and ball milled in a planetary ball mill at 240 rpm for 4 h using anhydrous ethanol as the ball milling medium and zirconium dioxide balls as the ball milling beads.
[0029] (3) Pre-sintering: The milled slurry was dried at 100 °C for 14 hours. The dried powder was sieved through a 60-mesh standard sieve and pre-sintered at 1400 °C for 4 hours at a heating rate of 5 °C per minute, and then cooled with the furnace.
[0030] (4) Secondary ball milling: The pre-burned powder is subjected to secondary ball milling. Most of the operations are the same as the primary ball milling, and the ball milling time is 8 hours.
[0031] (5) Granulation: The slurry after the secondary ball milling was dried at 100°C for 14 hours, and the dried powder was passed through a 60-mesh standard sieve. A 10 wt% PVA solution was used as a binder, and the mixture was fully mixed and passed through a 40-mesh standard sieve.
[0032] (6) Tabletting: Pour the granulated powder into a mold and make a green tablet with a diameter of 15 mm and a height of about 6 mm under a pressure of 4 MPa.
[0033] (7) Debinding: Debind the green body at 550 °C for 5 hours.
[0034] (8) Sintering: First, the temperature was rapidly increased to 1100 °C at a heating rate of 5 °C per minute, then the temperature was increased to 1550 °C at a heating rate of 3 °C per minute and sintered for 4 hours, then the temperature was decreased to 1100 °C at a cooling rate of 2 °C per minute, and then naturally cooled to room temperature to obtain a microwave dielectric ceramic sample.
[0035] The dielectric constant of this embodiment is 27.1, the dielectric loss is 102136 GHz, and the resonant frequency temperature coefficient is 16.7 ppm / °C.
[0036] Example 2
[0037] In this embodiment 2, Sr 1.6 La 0.4 Ti 0.6 Al 0.4 The preparation process of O4 microwave dielectric ceramics is referred to Example 1, except that: in this example, in step (1), x =0.4, that is, the ratio of raw materials is according to the chemical formula Sr 1.6 La 0.4 Ti 0.6 Al 0.4 O4 is weighed; the sintering temperature in step (8) is 1575 °C.
[0038] The dielectric constant of this embodiment is 22.5, the dielectric loss is 75464 GHz, and the resonant frequency temperature coefficient is -7.3 ppm / °C.
[0039] Example 3
[0040] In this embodiment 3, Sr 1.4La 0.6 Ti 0.4 Al 0.6 The preparation process of O4 microwave dielectric ceramics is referred to Example 1, except that: in this example, in step (1), x =0.6, that is, the ratio of raw materials is according to the chemical formula Sr 1.4 La 0.6 Ti 0.4 Al 0.6 O4 is weighed.
[0041] The dielectric constant of this embodiment is 20.3, the dielectric loss is 68282 GHz, and the resonant frequency temperature coefficient is -26.2 ppm / °C.
[0042] Example 4
[0043] In this embodiment 4, Sr 1.2 La 0.8 Ti 0.2 Al 0.8 The preparation process of O4 microwave dielectric ceramics is referred to Example 1, except that: in this example, in step (1), x =0.8, that is, the ratio of raw materials is according to the chemical formula Sr 1.2 La 0.8 Ti 0.2 Al 0.8 O4 is weighed.
[0044] The dielectric constant of this embodiment is 18.2, the dielectric loss is 59501 GHz, and the resonant frequency temperature coefficient is -38.2 ppm / °C.
[0045] Comparative Example 1
[0046] (1) Ingredient weighing: Weigh SrCO3 and TiO2 powders according to the stoichiometric ratio of Sr2TiO4.
[0047] (2) Primary ball milling: The weighed raw materials were transferred into a nylon ball mill jar, and ball milled in a planetary ball mill at 240 rpm for 4 h using anhydrous ethanol as the ball milling medium and zirconium dioxide balls as the ball milling beads.
[0048] (3) Pre-sintering: The milled slurry is dried at 100 °C for 14 hours. The dried powder is sieved through a 60-mesh standard sieve and pre-sintered at 1200 °C for 4 hours at a heating rate of 5 °C per minute, and then cooled with the furnace.
[0049] (4) Secondary ball milling: The pre-burned powder is subjected to secondary ball milling for 8 hours.
[0050] (5) Granulation: The dried powder is first passed through a 60-mesh standard sieve, and 10 wt% PVA solution is used as a binder. After fully mixing, the powder is passed through a 40-mesh standard sieve.
[0051] (6) Tabletting: Pour the granulated powder into a mold and make a green tablet with a diameter of 7 mm and a height of about 3 mm under a pressure of 4 MPa.
[0052] (7) Debinding: Debind the green body at 550 °C for 5 hours.
[0053] (8) Sintering: The temperature was raised to 1500 °C at a heating rate of 3 °C per minute and sintered for 4 hours. The temperature was then lowered to 1100 °C at a cooling rate of 2 °C per minute and then naturally cooled to room temperature to obtain a microwave dielectric ceramic sample.
[0054] The dielectric constant of this comparative example is 37.9, the dielectric loss is 70839 GHz, and the resonant frequency temperature coefficient is 142.1 ppm / °C.
[0055] Figure 1 The Sr2TiO4 prepared in Comparative Example 1 and the Sr2TiO4 prepared in Examples 1-4 are shown. 2-x La x Ti 1-x Al x O4(0.2≤ x ≤0.8) X-ray diffraction pattern of microwave dielectric ceramic materials, Figure 1 It can be seen that the prepared Sr 2-x La x Ti 1-x Al x O4(0.2≤ x ≤0.8) The microwave dielectric ceramic material presents a single tetragonal K2NiF4 structure.
[0056] Figure 2 and Figure 3 They are SEM images of Comparative Example 1 and Example 2, wherein Example 2 is preferably x =0.4 microwave dielectric ceramics. Figure 2 and Figure 3 It can be seen that x =0.4, the ceramic material has fewer pores, higher density, average grain size, and regular shape. The microwave dielectric ceramics with this composition have lower dielectric loss and higher quality factor.
[0057] The above descriptions are only some specific implementation methods of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any person familiar with the art within the technical scope disclosed in the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for preparing strontium titanate-based microwave dielectric ceramics, characterized in that: The chemical composition of the microwave dielectric ceramic is Sr 2-x La x Ti 1-x Al x O4, where 0.2≤ x ≤0.8; The microwave dielectric ceramic comprises the following steps: (1) According to Sr 2-x La x Ti 1-x Al x SrCO3, La2O3, Al2O3, and TiO2 are weighed in a stoichiometric ratio of O4, the weighed raw materials are mixed and then ball-milled, dried, sieved, and pre-calcined in sequence, and the powder obtained after pre-calcination is ball-milled for a second time and dried to obtain a powder; the pre-calcination process comprises the following steps: The temperature was raised to 1400°C at a rate of 5°C per minute, pre-fired at 1400°C for 4 hours, and then naturally cooled to room temperature; (2) granulating, sieving, tableting and debinding the powder obtained in step (1) to obtain a ceramic green body; (3) Sintering the green body obtained in step (2) at 1550°C-1575°C to obtain a microwave dielectric ceramic; the sintering process comprises the following steps: firstly heating the temperature to 1100°C at a heating rate of 5°C per minute, then heating the temperature to 1450°C-1600°C at a heating rate of 3°C per minute, and keeping the temperature for 4 hours; after the end of the heat preservation, cooling the temperature to 1100°C at a cooling rate of 2°C per minute, and then naturally cooling to room temperature to obtain a microwave dielectric ceramic; The relative dielectric constant of the microwave dielectric ceramic ε r =18.2~27.1, quality factor Q×f =59501~102136GHz, τ f =-38.2~16.7 ppm / ℃.
2. The method for preparing a strontium titanate-based microwave dielectric ceramic according to claim 1, characterized in that: x=0.4, the relative dielectric constant of the ceramic ε r =22.5, quality factor Q×f =75464 GHz, τ f =-7.3 ppm / ℃.
3. The method for preparing the strontium titanate-based microwave dielectric ceramic according to claim 1, characterized in that: In the step (1), the La2O3 is pre-treated by calcining at 900°C for 2 hours before being weighed.
4. The method for preparing the strontium titanate-based microwave dielectric ceramic according to claim 1, characterized in that: In the step (2), the specific process of the granulation includes: using a PVA solution with a concentration of 10 wt% as a binder, using a 60-mesh and 40-mesh standard sieves for sieving before and after the granulation, respectively, the tableting is dry pressing; and the debinding is calcining the ceramic green body at 550°C for 5 hours.