A kind of polypropylene material and its preparation method and application
By using highly crystalline copolymerized polypropylene resin and composite nucleating agent in polypropylene materials, combined with the dispersion effect of hydrotalcite, the problem of insufficient toughness of polypropylene materials under low temperature conditions is solved, and the material's high rigidity and low density are achieved. Suitable for automotive lightweight applications.
Patent Information
- Application Number
- CN202310320820.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Existing polypropylene materials have poor toughness under low temperature conditions, and in order to improve toughness, thermoplastic elastomers or talc powder are often added, resulting in an increase in material density and affecting lightweight and rigidity.
Highly crystalline copolymer polypropylene resin is used as the matrix, and composite nucleating agent and hydrotalcite are added. By regulating the ratio of α crystal form and β crystal form nucleating agent, a buffer zone is formed to improve the rigidity and toughness of the material, and through the formation of hydrotalcite Dispersion increases nucleation efficiency and reduces density.
It achieves the balance of high rigidity and high toughness of polypropylene materials under low temperature conditions, and increases the maximum energy absorption of low temperature multi-axis, making it suitable for lightweight automotive applications.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polypropylene materials, and in particular to a polypropylene material and a preparation method and application thereof. Background Art
[0002] Polypropylene material is one of the most widely used non-metallic materials in the automotive field. With the development of lightweight and high-performance automobiles, the requirements for material density, rigidity, toughness, and especially low-temperature toughness are becoming higher and higher.
[0003] Since the glass transition temperature of polypropylene (PP) material is around -20~-30℃, the low-temperature impact strength at -40℃ is low and the toughness is poor. Usually, in order to improve the low-temperature toughness of polypropylene materials, a large amount of thermoplastic elastomer needs to be added, but due to the presence of elastomer, its rigidity decreases. The rigidity of the material can be improved by a large amount of talcum powder, but the density increases, which is not conducive to the lightweight of the material. CN113354914A discloses a low-temperature blastable polypropylene composite material and its preparation method and application, with a talcum powder content of ≥15%, a high density, and is not conducive to lightweighting. CN106832600A uses a terpolymer as a modifier to improve the low-temperature toughness of polypropylene materials, but the terpolymer modifier is not easy to obtain, and there are components such as siloxane and acrylic acid that are incompatible with PP, which may cause incompatibility. Summary of the invention
[0004] The purpose of the present invention is to overcome the deficiencies of the above-mentioned prior art and provide a polypropylene material with low density, high rigidity and high low-temperature toughness, and a preparation method and application thereof.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A polypropylene material comprises the following components in parts by weight: 60-80 parts of a high-crystalline copolymer polypropylene resin, 5-10 parts of talc powder, 15-25 parts of a toughening agent, 2-4 parts of a composite nucleating agent, and 0-1 part of an auxiliary agent, wherein the composite nucleating agent comprises an α-crystal nucleating agent, a β-crystal nucleating agent, and hydrotalcite; the high-crystalline copolymer polypropylene resin has a crystallinity of 45%-58%.
[0007] The present invention has been found through experiments that copolymerized polypropylene with a crystallinity of 45%-58% is selected as a matrix, and the above-mentioned composite nucleating agent is added, which can generate high-strength α crystals under the induction of α nucleating agent, and can also form a small amount of β-crystals with loosely arranged wafers under the induction of β-nucleating agent, forming a buffer zone between high-strength α crystals and amorphous regions, and regulating the ratio of the two crystals by the ratio of the nucleating agent, thereby ensuring the rigidity of the material and improving the ability of the material to deform and absorb energy after receiving impact, thereby improving toughness. On the one hand, hydrotalcite, as a dispersant for the nucleating agent, can make the nucleating agent uniformly dispersed, play a better nucleation effect, have more and more uniform nucleation points, and have more refined grains, and both crystals are uniformly dispersed. On the other hand, hydrotalcite is distributed between the two nucleating agents, isolating them, inducing nucleation alone, avoiding the influence of the competition between the nucleating agents, and reducing the nucleation efficiency instead. The addition of a small amount of high-mesh talcum powder and toughening agent improves the rigidity and toughness of the material, making the material low in density, rigid-tough balance, and high in low-temperature multi-axis maximum absorption energy.
[0008] Preferably, the crystallinity of the high crystalline copolymer polypropylene resin is 48%-55%. When the crystallinity of the copolymer polypropylene resin meets the above requirements, it can better interact with the composite nucleating agent to improve the rigidity and toughness of the polypropylene material.
[0009] Preferably, the mass ratio of the α-crystal nucleating agent to the β-crystal nucleating agent in the composite nucleating agent is (1-2):1, and the total content of the α-crystal nucleating agent and the β-crystal nucleating agent in the composite nucleating agent is 8wt%-15wt%. The β-crystal nucleating agent induces PP to form a small amount of β-crystals with relatively loosely arranged crystals in the high-crystalline copolymer PP system, forming a buffer zone between the high-strength α-crystal and the amorphous region, and synergizing the toughening agent to enhance toughness, thereby greatly improving the toughness of the material. However, if the content of the β-crystal nucleating agent is too high, the rigidity cannot be improved. Hydrotalcite can accelerate the crystallization process and adjust the crystallization behavior of the resin. By controlling the ratio of the α-crystal nucleating agent and the β-crystal nucleating agent and the total content within the above range, it can be ensured that the polypropylene material has good rigidity and toughness.
[0010] Preferably, the α crystal nucleating agent is at least one of an aromatic acid metal soap α nucleating agent, a sorbitol α nucleating agent, a rosin α nucleating agent, and an organic phosphate α nucleating agent; the β crystal nucleating agent is at least one of an inorganic oxide β nucleating agent, an inorganic salt β nucleating agent, a condensed aromatic hydrocarbon β nucleating agent, an organic carboxylic acid and its salt β nucleating agent, an aromatic amide β nucleating agent, and a rare earth β nucleating agent; and the hydrotalcite is at least one of a magnesium aluminum hydrotalcite, a magnesium aluminum zinc hydrotalcite, and a calcium aluminum hydrotalcite.
[0011] The aromatic acid metal soap α nucleating agent is selected from at least one of the metal salts of aromatic carboxylic acids, sodium benzoate, aluminum benzoate, and aluminum p-tert-butylbenzoate; the sorbitol α nucleating agent is selected from at least one of dibenzylidene sorbitol, substituted dibenzylidene sorbitol, 1,3:2,4-di-p-methylbenzylidene sorbitol, and di-(3,4-dimethyldibenzylidene) sorbitol; the rosin α nucleating agent is selected from at least one of dehydroabietic acid, abietic acid salt, a mixture of abietic acid and its salts, and abietic amide; the organic phosphate α nucleating agent is selected from at least one of organic phosphate esters, organic phosphate basic metal salts, and composites.
[0012] The inorganic salt β-nucleating agent is selected from at least one of calcium silicate, calcium carbonate, and calcium sulfate; the condensed ring aromatic hydrocarbon β-nucleating agent is selected from at least one of quinacridone quinone, triphenothiazine, and disazo yellow; the organic carboxylic acid β-nucleating agent is selected from at least one of adipic acid dibenzoyl hydrazide and suberic acid; the organic carboxylate β-nucleating agent is selected from at least one of calcium tetrahydrophthalate, calcium suberate, calcium pimelate, polycarboxylic acid calcium salt, and polycarboxylic acid zinc salt; the aromatic amide β-nucleating agent is selected from at least one of 2,6-phthalic acid cyclohexylamide, 2,6-naphthalene dicarboxylic acid cyclohexylamide, and aromatic dicarbonamide; the rare earth β-nucleating agent is selected from at least one of rare earth lanthanide mononuclear metal compounds, rare earth multi-complexes, and binuclear complexes formed by rare earth and Group IIA metals; the inorganic oxide β-nucleating agent is selected from aluminum oxide.
[0013] Further preferably, the α-crystal nucleating agent is an organic phosphate α-nucleating agent, and the β-crystal nucleating agent is at least one of an aromatic amide β-nucleating agent and a rare earth β-nucleating agent. According to the experiment, the α-crystal nucleating agent and the β-crystal nucleating agent can synergistically improve the mechanical properties of the polypropylene material and increase the low-temperature multiaxial maximum absorption energy of the material; the hydrotalcite is calcium aluminum hydrotalcite.
[0014] Preferably, the preparation method of the composite nucleating agent is: mixing an α-crystal nucleating agent, a β-crystal nucleating agent and hydrotalcite to obtain a mixed powder, adding water to the mixed powder for extrusion granulation to obtain the composite nucleating agent; the amount of water added is 1.5 to 2.5 times that of the mixed powder, and the extrusion pressure is 0.5 to 7 MPa.
[0015] Preferably, the D50 particle size of the talc is ≤4.5 μm. Controlling the particle size of the talc within the above range can effectively increase the rigidity of the polypropylene material and ensure that the polypropylene material has a lower density.
[0016] Preferably, the toughening agent is at least one of ethylene-butene copolymer and ethylene-octene copolymer.
[0017] Preferably, the auxiliary agent is an antioxidant and a light stabilizer; the antioxidant comprises a primary antioxidant and a secondary antioxidant, the primary antioxidant is a hindered phenol antioxidant, such as antioxidant 1010, the secondary antioxidant is a thioether antioxidant, such as antioxidant 412s, and the light stabilizer is a hindered amine light stabilizer.
[0018] At the same time, the present invention also discloses a method for preparing the polypropylene material, which comprises the following steps:
[0019] (1) Mix the components uniformly according to the proportion to obtain a premix;
[0020] (2) Adding the premix into a twin-screw extruder, melt blending, extrusion granulation, and obtaining the polypropylene material.
[0021] The melt extrusion conditions of the twin-screw extruder are: zone one temperature 80-120°C, zone two temperature 180-200°C, zone three temperature 180-220°C, zone four temperature 180-220°C, zone five temperature 180-220°C, zone six temperature 180-220°C, zone seven temperature 180-220°C, zone eight temperature 180-220°C, zone nine temperature 180-220°C.
[0022] In addition, the invention also discloses the application of the polypropylene material in the field of preparing automobile instrument panels and automobile blasting pillars.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The invention uses high-crystalline copolymer polypropylene as a matrix resin, and significantly improves the rigidity and toughness of the polypropylene material by adding a composite nucleating agent. Meanwhile, by screening the components of the composite nucleating agent and further coordinating with talcum powder and a toughening agent, the mechanical properties of the polypropylene material are improved, and the low-temperature multi-axial maximum absorption energy of the polypropylene material is increased. Moreover, the polypropylene material has a lower density and is suitable for application in the fields of seamless airbag instrument panels for automobiles or pillars with side curtain blasting requirements. DETAILED DESCRIPTION
[0025] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0026] Unless otherwise specified, the materials used in the examples and comparative examples can be obtained through commercial channels. The materials used in the examples and comparative examples are as follows:
[0027] Highly crystalline copolymer polypropylene resin 1: PP EP5074X, China SABIC Petrochemical Co., Ltd., crystallinity 48%;
[0028] Highly crystalline copolymer polypropylene resin 2: PP BX3800, South Korea SK, crystallinity 55%;
[0029] Highly crystalline copolymer polypropylene resin 3: PP BI997, Hanwha Total Petrochemical, crystallinity 45%;
[0030] Highly crystalline copolymer polypropylene resin 4: PP BX3900, South Korea SK, crystallinity 58%;
[0031] Copolymer polypropylene resin 1: PP EP548R, CNOOC Shell Petrochemical Co., Ltd., crystallinity 41%;
[0032] Copolymer polypropylene resin 2: PP BX3920, South Korea SK, crystallinity 59.6%;
[0033] Homopolymer polypropylene resin: N-Z30S, Sinopec, crystallinity 48%;
[0034] Talc 1: HAR 3G77L, Shanghai Huazhongrong Industry and Trade Co., Ltd., 2.3 μm;
[0035] Talc 2: TYT-3000A, Guangzhou Tianyuan Chemical Co., Ltd., 4.5 μm;
[0036] Talc 3: HAR T84, Shanghai Huazhongrong Industry and Trade Co., Ltd., 2.0 μm;
[0037] Talc 4: TYT-777A, Haicheng Tianyuan Chemical Co., Ltd., 5.7 μm;
[0038] α-crystal nucleating agent 1: organic phosphate α-nucleating agent, TMP-6, di[2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate]hydroxyaluminum salt), Shanxi Chemical Industry Research Institute;
[0039] α-crystal nucleating agent 2: aromatic acid metal soap α-nucleating agent, NAR-6, sodium benzoate, Guangzhou Chenghe Technology Co., Ltd.;
[0040] α-crystal nucleating agent 3: sorbitol-based α-nucleating agent, NA-98, dibenzylidene sorbitol, Guangzhou Chenghe Technology Co., Ltd.;
[0041] α-crystal nucleating agent 4: rosin-based α-nucleating agent, KM-1600, dehydroabietic acid potassium salt, Arakawa Chemical, Japan;
[0042] β-crystal nucleating agent 1: aromatic amide β-nucleating agent, TMB-5, aromatic dicarbonamide, Shanxi Chemical Research Institute;
[0043] β-nucleating agent 2: rare earth β-nucleating agent, WBG-II, binuclear complex formed by rare earth and Group IIA metal, Guangdong Weilinna Functional Materials Co., Ltd.;
[0044] β-crystal nucleating agent 3: inorganic oxide β-nucleating agent, nano-alumina, Hebei Zhuyan Alloy Materials Co., Ltd.;
[0045] β-crystal nucleating agent 4: inorganic salt β-nucleating agent, nano calcium silicate, Tuoyi New Materials Co., Ltd.;
[0046] β-crystal nucleating agent 5: condensed aromatic hydrocarbon β-nucleating agent, γ-quinacridone (E3B), Clariant Chemicals (China) Co., Ltd.;
[0047] β-crystal nucleating agent 6: organic carboxylic acid β-nucleating agent, NAB-82, calcium tetrahydrophthalate, Guangzhou Chenghe Technology Co., Ltd.;
[0048] Hydrotalcite 1: calcium aluminum hydrotalcite, HG-100, Hunan Hengguang Technology Co., Ltd.;
[0049] Hydrotalcite 2: magnesium-aluminum hydrotalcite, AC-320, Chenghe Technology Co., Ltd.;
[0050] Hydrotalcite 3: magnesium aluminum zinc hydrotalcite, AZ-128, Chenghe Technology Co., Ltd.;
[0051] Toughener: POE ENGAGE 8842, The Dow Chemical Company;
[0052] Antioxidant: a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1, commercially available;
[0053] Light stabilizer: Hindered amine light stabilizer, commercially available.
[0054] The antioxidants and light stabilizers used in the examples and comparative examples are all the same commercially available products.
[0055] The crystallinity was tested by DSC method. A 10 mg sample was taken and heated to 220°C at a rate of 10°C / min in a nitrogen atmosphere, kept isothermal for 5 min, then cooled to room temperature at a rate of 10°C / min, and finally heated to 220°C at a rate of 10°C / min. As shown in formula (1), the ratio of the melting enthalpy of the second heating to the 100% crystallization enthalpy of polypropylene (209 J / g) is the crystallinity of polypropylene.
[0056] X ch = (△H f / △H0 f)×100% (1);
[0057] Where:X ch —Degree of crystallinity of the polymer measured by DSC method, %;
[0058] △H f — Melting enthalpy of polymer, J·g -1 ;
[0059] △H0 f—melting enthalpy of the polymer when the crystallinity is 100%, J.g -1 .
[0060] Example 1
[0061] An embodiment of the polypropylene material of the present invention, the formula of the polypropylene material of this embodiment is shown in Table 1, and the preparation method is as follows:
[0062] (1) Weighing an α-crystal nucleating agent, a β-crystal nucleating agent and hydrotalcite according to a ratio, stirring them evenly in a high-speed mixer, then adding water to the obtained powder mixture and stirring, wherein the weight of the water is twice the weight of the powder, and after the powder and water are evenly stirred, extruding granulation at an extrusion pressure of 5 MPa, and then drying the granules obtained by extrusion granulation to obtain the composite nucleating agent.
[0063] (2) Add high crystalline copolymer polypropylene resin, talcum powder, toughening agent, composite nucleating agent, antioxidant and light stabilizer into a high speed mixer and mix for 3 minutes to obtain a premix;
[0064] (3) adding the premix to the main feeding port of a twin-screw extruder for melt extrusion to obtain the polypropylene material; the melt extrusion conditions are: zone 1 temperature 100°C, zone 2 temperature 180°C, zone 3 temperature 200°C, zone 4 temperature 200°C, zone 5 temperature 200°C, zone 6 temperature 200°C, zone 7 temperature 200°C, zone 8 temperature 200°C, zone 9 temperature 200°C, and the aspect ratio of the screw is 40:1.
[0065] Embodiments 2 to 11
[0066] The embodiments of the polypropylene material of the present invention, the formulas of the polypropylene materials of Examples 2 to 11 are shown in Table 1, and the preparation method is the same as that of Example 1.
[0067] Comparative Examples 1 to 3
[0068] Comparative Examples 1 to 3 are polypropylene materials, the formulas of the polypropylene materials are shown in Table 1, and the preparation methods are the same as those of Example 1.
[0069] Table 1 (parts by weight)
[0070]
[0071] Example 12
[0072] An embodiment of the polypropylene material of the present invention, the formula of the polypropylene material in this embodiment is the same as that in embodiment 1, and the preparation method is as follows:
[0073] (1) Add high crystalline copolymer polypropylene resin, talc, toughening agent, α-crystal nucleating agent, β-crystal nucleating agent, hydrotalcite, antioxidant and light stabilizer into a high-speed mixer and mix for 3 minutes to obtain a premix;
[0074] (2) adding the premix to the main feeding port of a twin-screw extruder for melt extrusion to obtain the polypropylene material; the melt extrusion conditions are: zone 1 temperature 100°C, zone 2 temperature 180°C, zone 3 temperature 200°C, zone 4 temperature 200°C, zone 5 temperature 200°C, zone 6 temperature 200°C, zone 7 temperature 200°C, zone 8 temperature 200°C, zone 9 temperature 200°C, and the aspect ratio of the screw is 40:1.
[0075] Embodiments 13 to 15
[0076] The embodiments of the polypropylene material of the present invention, embodiments 13 to 15 are different from embodiment 1 only in that the types of high crystalline copolymer polypropylene resins are different, and the high crystalline copolymer polypropylene resins used in embodiments 13 to 15 are high crystalline copolymer polypropylene resins 2 to 4, respectively.
[0077] Embodiments 16 to 18
[0078] The embodiments of the polypropylene material of the present invention, embodiments 16 to 18 are different from embodiment 1 only in that the types of talcum powder are different, and the talcum powders used in embodiments 16 to 18 are talcum powders 2 to 4, respectively.
[0079] Embodiments 19 to 28
[0080] The embodiments of the polypropylene material of the present invention, embodiments 19 to 21 differ from embodiment 1 only in that the types of α crystal nucleating agents are different, namely α crystal nucleating agents 2 to 4; embodiments 22 to 26 differ from embodiment 1 only in that the types of β crystal nucleating agents are different, namely β crystal nucleating agents 2 to 6; embodiments 27 to 28 differ from embodiment 1 only in that the types of hydrotalcites are different, namely hydrotalcite 2 and hydrotalcite 3.
[0081] Comparative Examples 4 to 6
[0082] Comparative Examples 4 to 6 are polypropylene materials. The only difference between Comparative Examples 4 to 6 and Example 1 is that the high crystalline copolymer polypropylene resin 1 is replaced by copolymer polypropylene resin 1, copolymer polypropylene resin 2, and homopolymer polypropylene resin, respectively.
[0083] The performance tests were conducted on the polypropylene materials described in the examples and comparative examples. The test standards are as follows. The test results are shown in Table 2.
[0084] Tensile strength: Tested according to ISO527-1-2012, with a test speed of 50 mm / min and using 1A spline;
[0085] Simply supported beam notched impact strength: tested with reference to ISO179-2010, specimen size 80*10*4mm, notch machined, thickness retained at notch 8.0±0.2mm;
[0086] Flexural modulus: Tested according to ISO 178-2019, speed 2mm / min, specimen size 80*10*4mm;
[0087] Density: Tested in accordance with ISO1183-1-2019;
[0088] -40℃ multi-axial impact toughness rate and -40℃ multi-axial impact maximum absorbed energy: tested with reference to ASTM D3763-2010, impact velocity is 6.6m / s, impact head diameter is 12.7mm, support ring diameter is 76.2mm, and specimen size is 100*100*3mm.
[0089] Table 2
[0090] project Tensile strength (MPa) <![CDATA[Notched impact strength of simply supported beam (23 °C, kJ / m 2 )]]> <![CDATA[Notched impact strength of simply supported beam (-40 °C, kJ / m 2 )]]> Flexural modulus (MPa) <![CDATA[Density (g / cm 3 ).]]> -40℃ multiaxial impact toughness rate (%) -40℃ multi-axial impact maximum absorbed energy (J) Example 1 21.2 62.8 8.3 1816 0.953 100% 25.8 Example 2 20.9 72.3 9.2 1770 0.966 100% 26.2 Example 3 21.6 57.9 7.6 1760 0.945 100% 24.2 Example 4 21.6 60.8 8.0 1820 0.955 100% 25.5 Example 5 21.5 62.1 8.1 1795 0.957 100% 25.6 Example 6 19.2 69.8 9.3 1620 0.954 100% 22.1 Example 7 21.7 46.2 6.1 1860 0.954 60% 20.4 Example 8 20.9 62.1 7.9 1785 0.955 100% 25.1 Example 9 21.2 60.1 7.9 1810 0.953 100% 25.8 Example 10 21.7 48.2 6.1 1660 0.954 70% 20.4 Embodiment 11 20.1 51.4 7.1 1730 0.957 80% 21.6 Example 12 21.2 50.2 6.6 1720 0.954 70% 20.9 Example 13 21.3 60.3 8.1 1826 0.955 100% 25.6 Embodiment 14 20.8 63.3 8.4 1765 0.955 100% 24.3 Embodiment 15 21.4 56.2 7.7 1827 0.956 90% 23.4 Example 16 21.0 61.6 8.2 1776 0.956 100% 24.4 Embodiment 17 21.2 63.5 8.3 1825 0.953 100% 25.9 Embodiment 18 20.8 60.2 8.0 1480 0.952 90% 21.7 Embodiment 19 20.7 61.9 8.0 1746 0.956 100% 23.7 Embodiment 20 20.7 63.3 8.1 1725 0.956 100% 23.5 Embodiment 21 20.7 61.5 7.9 1693 0.956 100% 23.2 Embodiment 22 21.1 64.2 8.2 1808 0.957 100% 25.4 Embodiment 23 21.2 55.6 7.7 1815 0.957 90% 23.1 Embodiment 24 21.1 56.2 7.7 1826 0.954 90% 22.8 Embodiment 25 21.0 54.2 7.4 1802 0.956 80% 23.0 Embodiment 26 21.3 57.2 7.7 1790 0.955 100% 23.4 Embodiment 27 20.7 63.7 8.1 1716 0.957 100% 23.1 Embodiment 28 20.6 63.6 8.2 1720 0.956 100% 23.2 Comparative Example 1 20.2 50.4 5.8 1660 0.956 60% 19.5 Comparative Example 2 20.1 47.4 5.4 1705 0.957 60% 19.6 Comparative Example 3 20.8 59.8 7.7 1440 0.954 100% 19.8 Comparative Example 4 17.9 65.7 9.1 1320 0.953 100% 18.1 Comparative Example 5 21.6 45.2 4.8 1856 0.955 20% 17.9 Comparative Example 6 23.1 15.3 2.8 1910 0.956 0% 14.4
[0091] As can be seen from Table 2, the polypropylene materials described in Examples 1 to 28 all have good rigidity, toughness and strength, and the -40°C multi-axial impact toughness rate can reach more than 60%, the -40°C multi-axial impact maximum absorbed energy can reach more than 20J, and the density is relatively low, so they are suitable for use in fields such as automotive seamless airbag instrument panels or pillars with side curtain blasting requirements.
[0092] By comparing the formulas and test results of Examples 1 and 4 to 7, it can be found that the composition of the composite nucleating agent has a great influence on the performance of the polypropylene material. When the mass ratio of the α-crystalline nucleating agent to the β-crystalline nucleating agent in the composite nucleating agent is (1-2):1, the polypropylene material has good multiaxial impact performance, the -40°C multiaxial impact toughness rate can reach 100%, and the -40°C multiaxial impact maximum absorbed energy can reach more than 24J.
[0093] By comparing the formulas and test results of Examples 1 and 8 to 11, it can be found that when the total content of the α-crystal nucleating agent and the β-crystal nucleating agent in the composite nucleating agent is 8wt%-15wt%, the polypropylene material has better multiaxial impact performance. The unique layered bimetal of hydrotalcite has a good adsorption effect and can interact with the nucleating agent powder to fully disperse, which is conducive to better dispersion of the nucleating agent in the PP matrix, higher nucleation efficiency, and the crystals induced by the two nucleating agents are also finer and stacked on each other, so that rigidity and toughness are improved at the same time. When the content of the two crystal nucleating agents is low, the hydrotalcite will inhibit the effect of the nucleating agent, resulting in performance degradation; when the content of the two crystal nucleating agents is too high, the hydrotalcite is difficult to achieve the effect of uniform dispersion, and the two nucleating agents compete with each other and cannot achieve the effect of two crystals being fine and alternately uniformly dispersed, resulting in poor effect.
[0094] By comparing the preparation methods of Example 1 and Example 12, it can be found that the polypropylene material prepared using the composite nucleating agent obtained by extrusion granulation has significantly better low-temperature multiaxial impact performance.
[0095] By comparing the test results of Example 1 and Examples 13 to 15, it can be found that when the crystallinity of high crystalline polypropylene is 48%-58%, high-performance materials can be prepared, which have higher rigidity and toughness, and higher absorption energy; the crystallinity of Example 14 is relatively low, and the bending modulus is low, resulting in a low maximum absorption energy of -40°C multi-axial impact; the crystallinity of Example 15 is high, and the toughness is poor, which also leads to too low maximum absorption energy of -40°C multi-axial impact.
[0096] From the test results of Example 1 and Examples 16 to 18, it can be seen that when the particle size of talcum powder D50 is ≤4.5 μm, the comprehensive performance of the polypropylene material is relatively better, the modulus of Example 18 is greatly reduced, the material is soft, the absorbed energy is low during impact, and the maximum absorbed energy is reduced.
[0097] By comparing the test results of Example 1 and Examples 19 to 28, it can be found that the best effect is achieved when the organic phosphate α nucleating agent is compounded with an aromatic amide or rare earth β nucleating agent and calcium aluminum hydrotalcite. This is because different nucleating agents have different nucleating efficiencies, and when used in combination or when competing with each other, they can both achieve good stiffness and toughness enhancement effects.
[0098] Comparative Example 1 does not have hydrotalcite, and the nucleating agent cannot be well dispersed. Comparative Example 2 has a high content of composite nucleating agent and has agglomeration problems. Comparative Example 3 has a low talcum powder content and a very low modulus. The maximum absorbed energy of multi-axial impact at -40°C is only 19.8J. Comparative Example 4 uses ordinary copolymer PP, and the material has low rigidity and low absorbed energy. The PP matrix used in Comparative Example 5 has high crystallinity, low impact performance, and toughness of only 20%. The toughness of homopolymer PP is the worst, with 0% toughness fracture and absorbed energy of only 14.4J.
[0099] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A polypropylene material, characterized in that: The invention comprises the following components in parts by weight: 60-80 parts of high crystalline copolymer polypropylene resin, 5-10 parts of talc powder, 15-25 parts of toughening agent, 2-4 parts of composite nucleating agent, and 0-1 part of auxiliary agent, wherein the composite nucleating agent comprises α-crystal nucleating agent, β-crystal nucleating agent and hydrotalcite; the crystallinity of the high crystalline copolymer polypropylene resin is 45%-58%; the mass ratio of α-crystal nucleating agent to β-crystal nucleating agent in the composite nucleating agent is (1-2):1, and the total content of α-crystal nucleating agent and β-crystal nucleating agent in the composite nucleating agent is (1-2):
1. The amount is 8wt%-15wt%; the α crystal nucleating agent is at least one of an aromatic acid metal soap α nucleating agent, a sorbitol α nucleating agent, a rosin α nucleating agent, and an organic phosphate α nucleating agent; the β crystal nucleating agent is at least one of an inorganic oxide β nucleating agent, an inorganic salt β nucleating agent, a condensed aromatic hydrocarbon β nucleating agent, an organic carboxylic acid and its salt β nucleating agent, an aromatic amide β nucleating agent, and a rare earth β nucleating agent; the hydrotalcite is at least one of a magnesium aluminum hydrotalcite, a magnesium aluminum zinc hydrotalcite, and a calcium aluminum hydrotalcite.
2. The polypropylene material according to claim 1, characterized in that The high crystalline copolymer polypropylene resin has a crystallinity of 48%-55%.
3. The polypropylene material according to claim 1, characterized in that The α crystal nucleating agent is an organic phosphate α nucleating agent, the β crystal nucleating agent is at least one of an aromatic amide β nucleating agent and a rare earth β nucleating agent; and the hydrotalcite is calcium aluminum hydrotalcite.
4. The polypropylene material according to claim 1, characterized in that The preparation method of the composite nucleating agent comprises: uniformly mixing an α-crystal nucleating agent, a β-crystal nucleating agent and hydrotalcite, adding water and performing extrusion granulation to obtain the composite nucleating agent.
5. The polypropylene material according to claim 1, characterized in that The D50 particle size of the talc is ≤4.5 μm.
6. The polypropylene material according to claim 1, characterized in that The toughening agent is at least one of ethylene-butene copolymer and ethylene-octene copolymer, and the auxiliary agent is an antioxidant and a light stabilizer.
7. A method for preparing the polypropylene material according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (1) uniformly mixing the components according to a proportion to obtain a premix; (2) adding the premix into a twin-screw extruder, melt blending, extruding and granulating to obtain the polypropylene material.
8. Use of the polypropylene material according to any one of claims 1 to 6 in the preparation of automobile instrument panels and automobile blasting pillars.
Citation Information
Patent Citations
Ultralow temperature-resistant polypropylene composition and preparation method thereof
CN106832600A
Polypropylene composite material capable of blasting at low temperature, preparation method and application thereof
CN113354914A
A material and composition for reducing blood pressure
EP0005074A1
Polypropylene composition
CN106397988A
Application of nucleating agent for lowering separation viscidity of polypropylene composite material
CN109354773A