A method for forming a low-temperature shear deformation layer on the surface of a TC4 titanium alloy workpiece

By sliding and frictional treatment of TC4 titanium alloy workpieces under low temperature environments, the low-temperature shear deformation layer is formed, which solves the problem of insufficient wear resistance of titanium alloy parts, significantly improves hardness and wear resistance, and is suitable for titanium of different sizes Alloy components and reduce costs and equipment requirements.

CN116219339BActive Publication Date: 2024-11-22SHAANXI RAILWAY LOGISTICS GRP CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211648225.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-11-22
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

The surface coating of titanium alloy parts is prone to fall off under low temperature environments, resulting in insufficient wear resistance and limiting their application in the aerospace field.

Method used

The surface of TC4 titanium alloy workpiece is treated by low-temperature shear deformation method. By contacting the titanium alloy workpiece with the grinding workpiece and sliding and friction under a low-temperature environment, a low-temperature shear deformation layer is formed to enhance surface hardness and wear resistance.

Benefits of technology

It significantly improves the hardness and wear resistance of titanium alloys, forms a stable gradient structure, enhances the surface performance of the material, and is suitable for titanium alloy parts of different sizes, reducing costs and equipment requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116219339B_ABST
    Figure CN116219339B_ABST
Patent Text Reader

Abstract

The present invention provides a method for forming a low-temperature shear deformation layer on the surface of a TC4 titanium alloy workpiece, which comprises the following steps: 1) contacting the TC4 titanium alloy workpiece with a counter-grinding workpiece to form a friction area; 2) reducing the ambient temperature of the TC4 titanium alloy workpiece and the counter-grinding workpiece to a low temperature; 3) causing the TC4 titanium alloy workpiece and the counter-grinding workpiece to undergo sliding friction to obtain a TC4 titanium alloy workpiece with a surface having a low-temperature shear deformation layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal coatings, and in particular to a method for forming a low-temperature shear deformation layer on the surface of a TC4 titanium alloy workpiece. Background Art

[0002] Titanium alloy has excellent comprehensive properties such as high specific strength, low density, good corrosion resistance, and good low-temperature mechanical properties. In recent years, it has become a key material for manufacturing rocket fuel tanks, impeller brackets, cryogenic fasteners and other parts. However, the oxide layer formed on the surface will significantly reduce the surface hardness and wear resistance of titanium alloys, thus restricting its application in the aerospace field. Although existing surface strengthening technologies such as laser shot peening, ion nitriding, and composite coatings can effectively enhance the surface properties of titanium alloys, there are problems of expensive equipment and high technical difficulty in the implementation process. In addition, when using the surface coating method, the coating and the substrate are easy to fall off in a low-temperature environment, thereby aggravating the wear of titanium alloy parts. Summary of the invention

[0003] One of the present inventions provides a method for forming a low-temperature shear deformation layer on the surface of a TC4 titanium alloy workpiece, which comprises the following steps:

[0004] 1) The TC4 titanium alloy workpiece is brought into contact with the counter-grinding workpiece to form a friction area;

[0005] 2) Lower the ambient temperature of the TC4 titanium alloy workpiece and the grinding workpiece to low temperature;

[0006] 3) The TC4 titanium alloy workpiece is subjected to sliding friction with a counter-grinding workpiece to obtain a TC4 titanium alloy workpiece having a low-temperature shear deformation layer on its surface.

[0007] In a specific embodiment, the contact pressure between the TC4 titanium alloy workpiece and the grinding workpiece is 50 to 200N.

[0008] In a specific embodiment, the low temperature is -120°C to -180°C.

[0009] In a specific embodiment, the sliding friction rate is 0.1 to 2 m / s.

[0010] In a specific embodiment, the sliding friction time is 0.5 to 2 hours.

[0011] In a specific embodiment, before the sliding friction is performed, the TC4 titanium alloy workpiece and the counter-grinding workpiece are kept at a low temperature for more than 0.5 h.

[0012] In a specific embodiment, the ambient temperature is lowered to the low temperature at a cooling rate of 5 to 10° C. / min.

[0013] In a specific embodiment, the contact pressure between the TC4 titanium alloy workpiece and the grinding workpiece is 200N; before the sliding friction, the TC4 titanium alloy workpiece and the grinding workpiece are kept at a low temperature for 0.5h; the low temperature is -160°C; the sliding friction rate is 0.5m / s; and the sliding friction time is 1h.

[0014] In a specific embodiment, the surface morphology of the TC4 titanium alloy workpiece is one of a plane, a spherical surface, an arc surface and a cylindrical surface.

[0015] The chemical composition of the TC4 titanium alloy of the present invention is as follows: 5.5wt% to 6.75wt% of aluminum (Al), 3.5wt% to 4.5wt% of vanadium (V), less than or equal to 0.40wt% of iron (Fe), less than or equal to ≤0.08wt% of carbon (C), less than or equal to 0.05wt% of nitrogen (N), less than or equal to 0.015wt% of hydrogen (H), less than or equal to 0.20wt% of oxygen (O), and the rest is titanium (Ti). Beneficial effects of the present invention:

[0016] The present invention aims to solve the problem of insufficient wear resistance of titanium alloy parts during use, and uses low-temperature shear deformation to strengthen the surface properties of titanium alloy parts to obtain a low-temperature shear deformation layer. The low-temperature shear deformation layer can effectively inhibit the initiation and expansion of cracks through the dislocation strengthening effect, significantly improve the surface properties such as hardness and wear resistance of titanium alloy, and show excellent work hardening effect. The low-temperature shear deformation method proposed in the present invention can uniformly regulate the sub-surface microstructure of the material, and the formed gradient structure has obvious transition characteristics, so it has a more stable improvement effect compared with the existing surface coating technology. In addition, the low-temperature shear deformation method of the present invention is suitable for titanium alloy parts of different sizes, so the low-temperature shear deformation method proposed in the present invention has obvious advantages in cost control and application range. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The microstructures of the longitudinal sections of the TC4 titanium alloy workpieces of Example 1 and Comparative Examples 1 to 3 are shown.

[0018] Figure 2 The wear morphologies of the worn surfaces of the TC4 titanium alloy workpieces of Example 1 and Comparative Examples 1 to 3 after the wear resistance test are shown. DETAILED DESCRIPTION

[0019] The present invention will be further described below in conjunction with examples, but the examples of the present invention are only exemplary descriptions, and the implementation methods do not constitute limitations of the present invention under any circumstances.

[0020] Example 1

[0021] The titanium alloy workpiece used is TC4 titanium alloy, and its chemical composition is as follows (wt.%): aluminum (Al) = 5.50, vanadium (V) = 4.00, iron (Fe) = 0.30, carbon (C) = 0.06, nitrogen (N) = 0.03, hydrogen (H) = 0.010, oxygen (O) = 0.10, and the rest is titanium (Ti). The surface of the workpiece is a flat morphology.

[0022] The grinding workpiece used is GCr15 bearing steel, and its chemical composition is as follows (wt.%): carbon (C) = 0.99, silicon (Si) = 0.17, manganese (Mn) = 0.33, phosphorus (P) = 0.012, sulfur (S) = 0.0014, chromium (Cr) = 1.57, copper (Cu) = 0.074, nickel (Ni) = 0.024, and the rest is iron (Fe). The surface of the grinding workpiece is a plane morphology matched with the surface of the titanium alloy workpiece.

[0023] 1) Install the TC4 titanium alloy workpiece on the rotating shaft of the friction mechanism of the dry friction and wear testing machine, and install the counter-grinding workpiece on the fixed shaft of the friction mechanism;

[0024] 2) The TC4 titanium alloy workpiece is brought into contact with the counter-grinding workpiece through a hydraulic transmission system to form a friction area;

[0025] 3) Place the TC4 titanium alloy workpiece and the counter-grinding workpiece in a low-temperature environment box, close the box door, and form a closed friction and wear environment;

[0026] 4) Adjust the contact pressure between the TC4 titanium alloy workpiece and the grinding workpiece to 200N

[0027] 5) Lower the temperature in the low temperature environment box to -160°C at a cooling rate of 7°C / min and keep it warm for 0.5h;

[0028] 6) The TC4 titanium alloy workpiece and the counter-wear workpiece are subjected to sliding friction wear at a temperature of -160°C, a sliding friction rate of 0.5 m / s, and a sliding time of 1 h to achieve shear deformation on the surface of the titanium alloy workpiece, thereby obtaining a TC4 titanium alloy workpiece having a low-temperature shear deformation layer on the surface.

[0029] Example 2

[0030] The titanium alloy workpiece and the grinding workpiece used are the same as those in Example 1.

[0031] 1) Install the TC4 titanium alloy workpiece on the rotating shaft of the friction mechanism of the dry friction and wear testing machine, and install the counter-grinding workpiece on the fixed shaft of the friction mechanism;

[0032] 2) The TC4 titanium alloy workpiece is brought into contact with the counter-grinding workpiece through a hydraulic transmission system to form a friction area;

[0033] 3) Place the TC4 titanium alloy workpiece and the counter-grinding workpiece in a low-temperature environment box, close the box door, and form a closed friction and wear environment;

[0034] 4) Adjust the contact pressure between the TC4 titanium alloy workpiece and the grinding workpiece to 50N;

[0035] 5) Lower the temperature in the low temperature environment box to -180°C at a cooling rate of 5°C / min and keep it warm for 0.5h;

[0036] 6) The TC4 titanium alloy workpiece and the counter-wear workpiece are subjected to sliding friction wear at a temperature of -180°C, a sliding friction rate of 0.1 m / s, and a sliding time of 0.5 h to achieve shear deformation on the surface of the titanium alloy workpiece, thereby obtaining a TC4 titanium alloy workpiece having a low-temperature shear deformation layer on the surface.

[0037] Example 3

[0038] The titanium alloy workpiece and the grinding workpiece used are the same as those in Example 1.

[0039] 1) Install the TC4 titanium alloy workpiece on the rotating shaft of the friction mechanism of the dry friction and wear testing machine, and install the counter-grinding workpiece on the fixed shaft of the friction mechanism;

[0040] 2) The TC4 titanium alloy workpiece is brought into contact with the counter-grinding workpiece through a hydraulic transmission system to form a friction area;

[0041] 3) Place the TC4 titanium alloy workpiece and the counter-grinding workpiece in a low-temperature environment box, close the box door, and form a closed friction and wear environment;

[0042] 4) Adjust the contact pressure between the TC4 titanium alloy workpiece and the grinding workpiece to 200N;

[0043] 5) Lower the temperature in the low temperature environment box to -120°C at a cooling rate of 10°C / min and keep it warm for 0.5h;

[0044] 6) The TC4 titanium alloy workpiece and the counter-wear workpiece are subjected to sliding friction wear at a temperature of -120°C, a sliding friction rate of 2 m / s, and a sliding time of 2 h to achieve shear deformation on the surface of the titanium alloy workpiece, thereby obtaining a TC4 titanium alloy workpiece having a low-temperature shear deformation layer on the surface.

[0045] Comparative Example 1

[0046] The titanium alloy workpiece and the grinding workpiece used are the same as those in Example 1.

[0047] The difference from Example 1 is step 5), which is as follows:

[0048] 1) Install the TC4 titanium alloy workpiece on the rotating shaft of the friction mechanism of the dry friction and wear testing machine, and install the counter-grinding workpiece on the fixed shaft of the friction mechanism;

[0049] 2) The TC4 titanium alloy workpiece is brought into contact with the counter-grinding workpiece through a hydraulic transmission system to form a friction area;

[0050] 3) Place the TC4 titanium alloy workpiece and the counter-grinding workpiece in a low-temperature environment box, close the box door, and form a closed friction and wear environment;

[0051] 4) The contact pressure between the TC4 titanium alloy workpiece and the counter-grinding workpiece was adjusted to 200 N, the sliding friction rate was set to 0.5 m / s on the friction and wear testing machine, and the sliding time was set to 1 h;

[0052] 5) Lower the temperature in the low temperature environment box to -100°C at a rate of 7°C / min and keep it warm for 0.5h;

[0053] 6) The TC4 titanium alloy workpiece and the counter-wear workpiece are subjected to sliding friction wear at a temperature of -100°C, a sliding friction rate of 0.5 m / s, and a sliding time of 1 h to achieve shear deformation on the surface of the titanium alloy workpiece, thereby obtaining a TC4 titanium alloy workpiece having a low-temperature shear deformation layer on the surface.

[0054] Comparative Example 2

[0055] The titanium alloy workpiece and the grinding workpiece used are the same as those in Example 1.

[0056] The difference from Example 2 is step 4), which is as follows:

[0057] 1) Install the TC4 titanium alloy workpiece on the rotating shaft of the friction mechanism of the dry friction and wear testing machine, and install the counter-grinding workpiece on the fixed shaft of the friction mechanism;

[0058] 2) The TC4 titanium alloy workpiece is brought into contact with the counter-grinding workpiece through a hydraulic transmission system to form a friction area;

[0059] 3) Place the TC4 titanium alloy workpiece and the counter-grinding workpiece in a low-temperature environment box, close the box door, and form a closed friction and wear environment;

[0060] 4) Adjust the contact pressure between the TC4 titanium alloy workpiece and the grinding workpiece to 30N;

[0061] 5) Lower the temperature in the low temperature environment box to -180°C at a cooling rate of 5°C / min and keep it warm for 0.5h;

[0062] 6) The TC4 titanium alloy workpiece and the counter-wear workpiece are subjected to sliding friction wear at a temperature of -180°C, a sliding friction rate of 0.1 m / s, and a sliding time of 0.5 h to achieve shear deformation on the surface of the titanium alloy workpiece, thereby obtaining a TC4 titanium alloy workpiece having a low-temperature shear deformation layer on the surface.

[0063] Comparative Example 3

[0064] The titanium alloy workpiece and the grinding workpiece used are the same as those in Example 1.

[0065] The difference from Example 3 is that step 3) and step 5) of Example 3 are omitted, which are as follows:

[0066] 1) Install the TC4 titanium alloy workpiece on the rotating shaft of the friction mechanism of the dry friction and wear testing machine, and install the counter-grinding workpiece on the fixed shaft of the friction mechanism;

[0067] 2) The TC4 titanium alloy workpiece is brought into contact with the counter-grinding workpiece through a hydraulic transmission system to form a friction area;

[0068] 3) Adjust the contact pressure between the TC4 titanium alloy workpiece and the grinding workpiece to 200N;

[0069] 4) The TC4 titanium alloy workpiece and the counter-wear workpiece are subjected to sliding friction wear at an ambient temperature, a sliding friction rate of 2 m / s, and a sliding time of 2 h to achieve shear deformation on the surface of the titanium alloy workpiece, thereby obtaining a TC4 titanium alloy workpiece having a common shear deformation layer on the surface.

[0070] Performance measurement

[0071] (1) Microstructure detection

[0072] The wire cutting method was used to cut along the direction perpendicular to the low temperature shear deformation layer of Examples 1 to 3 and Comparative Examples 1 and 2 and the normal shear deformation layer of Comparative Example 3, and the microstructure of the longitudinal section was observed by optical microscope (Olympus BX53M) for characterization and analysis. The microstructure of the longitudinal section of Example 1 and Comparative Examples 1 to 3 is as follows: Figure 1 The distance between the dotted line and the upper boundary indicates the degree of plastic deformation of the longitudinal section of the specimen.

[0073] from Figure 1It can be seen that the microstructure of the TC4 titanium alloy sample is a typical α+β two-phase structure, in which the α phase is equiaxed and the β phase is dispersed in the microstructure. Among them, the plastic deformation of Example 1 is small, and there is obvious grain refinement in the low-temperature shear deformation layer, which is more dense and shows work hardening characteristics; while the grain refinement and densification effects of Comparative Examples 1 and 2 are reduced, and the plastic deformation of Comparative Example 3 is large, which is related to the thermal softening of the material surface during reciprocating sliding under room temperature shear deformation conditions. The results show that the low-temperature shear deformation method proposed in the present invention can form a low-temperature shear deformation layer with a work hardening effect on the surface of the titanium alloy, inhibit the generation of surface cracks, and thus enhance the surface properties of the titanium alloy such as hardness and wear resistance.

[0074] (2) Hardness test

[0075] The hardness of the TC4 titanium alloy workpieces with low-temperature shear deformation layers on the surfaces obtained in Examples 1 to 3 and Comparative Examples 1 and 2 and the TC4 titanium alloy workpieces with ordinary shear deformation layers on the surfaces obtained in Comparative Example 3 were tested in accordance with GB / T4340.1-2012 "Vickers Hardness Test for Metallic Materials - Test Methods". The results are shown in Table 1.

[0076] As can be seen from Table 1, the hardness of Examples 1 to 3 is improved compared with Comparative Examples 1 to 3, among which Example 1 has the highest hardness. Compared with Example 1, the changes in ambient temperature and contact pressure parameters of Examples 2 and 3 slightly reduce the hardness, while the processing condition of Comparative Example 3 is ambient temperature shear deformation, and the hardness is the lowest. This result shows that the low-temperature shear deformation method proposed in the present invention can improve the hardness of the titanium alloy surface.

[0077] (3) Wear resistance test

[0078] Pin-disc friction and wear tests were carried out on the TC4 titanium alloy workpieces with low-temperature shear deformation layer on the surfaces obtained in Examples 1 to 3 and Comparative Examples 1 and 2, and the TC4 titanium alloy workpiece with ordinary shear deformation layer on the surfaces obtained in Comparative Example 3. The tests were carried out on a MMU-10G high-temperature end face friction and wear testing machine with a loading force of 200 N, a rotation speed of 200 r / min, a test time of 0.5 h, and the grinding material was GCr15 bearing steel.

[0079] 1) Weigh the specimen before wear and record it as M1;

[0080] 2) The test was carried out on a MMU-10G high-temperature end face friction and wear testing machine. The grinding material was GCr15 bearing steel, the loading force was 200N, the speed was 200r / min, and the test time was 0.5h. The worn specimens were cleaned, dried, and weighed, which was calculated as M2;

[0081] 3) Calculate the wear amount by subtracting M2 from M1. The results are shown in Table 1.

[0082] The wear morphology of the worn surfaces of the TC4 titanium alloy workpieces of Example 1 and Comparative Examples 1 to 3 after the wear resistance test was observed using a scanning electron microscope (Hitachi SU1510). Figure 2 shown.

[0083] As can be seen from Table 1, the wear amount of Examples 1 to 3 is reduced compared with Comparative Examples 1 to 3, among which Example 1 has the lowest wear amount, while Comparative Example 3, which is processed under room temperature shear deformation, has the highest wear amount. This result shows that the low-temperature shear deformation method proposed in the present invention can enhance the wear resistance of titanium alloys.

[0084] from Figure 2 It can be seen that the surface of Example 1 is relatively smooth without obvious damage, the surfaces of Comparative Examples 1 and 2 have a certain degree of damage, and the surface of Comparative Example 3 has a large area of ​​chipping and peeling.

[0085] Table 1

[0086] Example Hardness / HV Wear resistance (wear amount / mg) Example 1 360 49 Example 2 348 60 Example 3 350 56 Comparative Example 1 332 81 Comparative Example 2 325 80 Comparative Example 3 217 115

[0087] Although the present invention has been described with reference to specific embodiments, it will be appreciated by those skilled in the art that various changes may be made without departing from the true spirit and scope of the present invention. In addition, the subject matter, spirit and scope of the present invention may be varied to accommodate specific situations, materials, material combinations and methods. All of these changes are included within the scope of the claims of the present invention.

Claims

1. A method for forming a low-temperature shear deformation layer on the surface of a TC4 titanium alloy workpiece, comprising the following steps: 1) The TC4 titanium alloy workpiece is brought into contact with the counter-grinding workpiece to form a friction area; 2) lowering the ambient temperature of the TC4 titanium alloy workpiece and the counter-grinding workpiece to a low temperature, the low temperature being -120°C to -180°C, at a cooling rate of 5 to 10°C / min; 3) The TC4 titanium alloy workpiece is subjected to sliding friction with the counter-grinding workpiece to obtain a TC4 titanium alloy workpiece with a low-temperature shear deformation layer on the surface, wherein: The contact pressure between the TC4 titanium alloy workpiece and the counter-grinding workpiece is 50 to 200 N, the sliding friction rate is 0.1 to 2 m / s, and the sliding friction time is 0.5 to 2 h; Wherein, before the sliding friction is performed, the TC4 titanium alloy workpiece and the counter-grinding workpiece are kept at a low temperature for more than 0.5 h.

2. The method according to claim 1, characterized in that: The contact pressure between the TC4 titanium alloy workpiece and the counter-grinding workpiece is 200N; before the sliding friction, the TC4 titanium alloy workpiece and the counter-grinding workpiece are kept at a low temperature for 0.5h; the low temperature is -160°C; the sliding friction rate is 0.5m / s; and the sliding friction time is 1h.

Citation Information

Patent Citations

  • Titanium alloy low temperature carbonitriding simultaneous aging technique with ageing strengthening effect

    CN108396283A

  • Processing method for improving low-temperature superplasticity of Ti-6Al-4V alloy

    CN108677116A

  • Method of chemically plating nickel, boron and lead high hardness wear-resistant coating to surface of titanium alloy

    CN109852955A

  • Titanium alloy for wearable / friction material

    CN1827812A

  • Production method for titanium alloy thread part and titanium alloy thread part using the same

    JP2003129215A