A method for enriching cobalt from nickel-iron alloy using Curie temperature

By using a combination of oxidation slagging, carbon supplementation and crystal inducer in nickel-iron alloy, and using the high Curie point characteristics of cobalt for segregation crystallization and magnetic adsorption, the problem of difficulty in cobalt separation and environmental pollution after smelting of laterite nickel ore is solved. It achieves efficient enrichment and separation of cobalt, which is suitable for the needs of the new energy automobile industry.

CN116240444BActive Publication Date: 2024-10-01GANSU GOLDEN PIED MONTAND SILVER PEAKS (GPASP) METALLURGICL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211692450.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-10-01
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

Existing technology cannot effectively separate cobalt from cobalt-containing nickel-iron alloys after smelting laterite nickel ore, resulting in high cobalt smelting process costs, serious environmental pollution, and difficulty in meeting the demand for cobalt resources for new energy vehicles.

Method used

The Curie temperature method is used to oxidize slagging, carbon supplement and crystal inducer in the nickel-iron alloy, and utilize the high Curie point characteristics of cobalt for segregation crystallization and magnetic adsorption to achieve enrichment and separation of cobalt.

Benefits of technology

It achieves efficient enrichment and separation of cobalt, reduces process costs, reduces equipment investment and environmental pollution, has a wide range of applications, and is suitable for the needs of the new energy automobile industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116240444B_ABST
    Figure CN116240444B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of metallurgy technology, and its purpose is to provide a method for enriching cobalt from nickel-iron alloy by using Curie temperature, and the different Curie temperature of each metal element in the nickel-iron alloy containing cobalt after pyrometallurgy of laterite nickel ore is used, and the nickel-iron alloy is crystallized near the Curie temperature of cobalt during the cooling and crystallization process after melting, and a cobalt-friendly crystallization inducer is added to induce cobalt to segregate and magnetically adsorb, so that the cobalt in the alloy is finally enriched at the bottom of the iron ladle, so as to achieve the purpose of enriching and separating cobalt. The present invention optimizes the existing cobalt smelting process, has the advantages of low cost, small equipment investment, energy saving and environmental protection, and can be enriched to different cobalt contents for direct use according to the needs of downstream industries, solves the problems of difficulty, high cost and great environmental harm in the enrichment and separation of cobalt in the existing cobalt-containing nickel-iron alloy, plays a great role in promoting the new energy vehicle industry, and has good economic benefits and broad market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, is suitable for enriching and separating cobalt from a cobalt-containing nickel-iron alloy product smelted by pyrometallurgy of laterite nickel ore, and specifically relates to a method for enriching cobalt from the nickel-iron alloy by utilizing Curie temperature. Background Art

[0002] As the global energy system gradually reduces its dependence on fossil raw materials, major automakers are turning from fuel vehicles to electric vehicles in response to climate change. The batteries of electric vehicles are currently: ternary lithium batteries, lithium iron phosphate batteries, and nickel-metal hydride batteries. Among them, nickel-metal hydride batteries are the most stable, lithium iron phosphate batteries are the safest, and ternary lithium batteries have the largest power. The common positive electrode materials of ternary batteries are 523 (composition is 50% nickel, 20% cobalt, 30% manganese), 622 (composition is 60% nickel, 20% cobalt, 20% manganese) and 811 (composition is 80% nickel, 10% cobalt, 10% manganese). Cobalt is used as the positive electrode material of ternary lithium batteries for electric vehicles, which can significantly improve the material's cycle and rate performance, that is, battery life. As one of the positive electrode materials of ternary lithium batteries, cobalt has become a rare metal resource due to its scarcity, resulting in limited reserves and rising prices. The price exceeded 650,000 yuan / ton in 2018, and the high price in 2021 also exceeded 550,000 yuan / ton. The high price has become a constraint on the development of new energy vehicles.

[0003] Cobalt ore rarely exists alone. It is mainly associated with nickel ore, copper ore, pyrite and arsenic deposits, and the content is relatively small, so it is relatively difficult to extract. Cobalt ore resources mainly include five types: nickel-cobalt sulfide ore, laterite nickel ore (oxide ore), copper-cobalt ore, arsenic-cobalt ore and cobalt-containing pyrite. The characteristics of cobalt smelting are low raw material grade, long extraction process and multiple extraction methods. The process of extracting cobalt from traditional nickel sulfide ore is mostly to extract nickel, copper and other resources in the pre-process, and then continue to extract cobalt by wet method. The cobalt extraction process examples are as follows:

[0004] Extracting cobalt from nickel, copper and sulfur converting slag: The cobalt-containing converting slag is subjected to reduction sulfidation smelting in a blast furnace or electric furnace to obtain cobalt alloy or cobalt matte; after magnetic separation and enrichment, it is pressurized and acid-leached to allow the cobalt to enter the solution; after the solution is purified, oxalic acid is added to cause the cobalt to produce cobalt oxalate precipitate, and the cobalt oxalate can be calcined to produce refined cobalt oxide products.

[0005] Extracting cobalt from nickel refining and purification slag: The cobalt slag produced by the purification of the anode liquid in the process of nickel electrolytic refining is an important raw material for cobalt extraction. The cobalt slag is leached with reducing sulfuric acid to make the cobalt enter the solution in the form of cobalt sulfate. The solution is iron-removed by the sodium ferroaluminate method, and impurities such as copper, zinc, and manganese are removed by extraction. Pure cobalt chloride solution is obtained by separating nickel and cobalt, thereby producing cobalt oxide products, or obtaining metallic cobalt by electrolysis.

[0006] Extracting cobalt from cobalt-containing pyrite: Cobalt-containing pyrite can produce cobalt-sulfur concentrate containing 0.3% to 0.5% cobalt after flotation. The cobalt-sulfur concentrate is roasted by sulfuric acid to convert valuable elements such as cobalt, nickel, and copper in the concentrate into soluble sulfates. The roasted sand is leached with water or acid to transfer cobalt, nickel, copper, etc. into the solution; the leached solution is purified to remove impurities such as iron, copper, zinc, and manganese, and then separated by nickel and cobalt to obtain a pure cobalt solution, which is then used to produce metallic cobalt by electrolysis.

[0007] Extracting cobalt from arsenic-cobalt ore: Arsenic-cobalt ore is roasted or smelted to volatilize and remove arsenic as As2O3, and roasted sand or cobalt matte is obtained. The cobalt enters the solution through acid leaching. The solution is then separated from nickel and cobalt after removing iron, arsenic, copper, zinc, manganese and other impurities. The purified cobalt solution is then used to produce metallic cobalt or cobalt oxide products according to market demand.

[0008] Extracting cobalt from laterite nickel ore: Indonesia has the richest reserves of laterite nickel ore resources. The High Pressure Acid Leach (HPAL) process can process Indonesia's low-grade laterite nickel ore and recover the valuable element cobalt, but its acid consumption is high and the tailings pollution is serious.

[0009] From the above processes, the cobalt smelting process can be roughly divided into five categories, all of which are wet processes: wet extraction of cobalt after high-temperature smelting enrichment, leaching of cobalt after sulfuric acid roasting, reduction roasting ammonia leaching and pressure leaching.

[0010] Since the existing technology is not capable of beneficiating laterite nickel ore, the wet leaching process involves whole-ore leaching. The cobalt content in laterite nickel ore is generally 0.01-0.1wt%. It is conceivable how much ore and reagent resources are consumed to extract one ton of cobalt, and how much tailings are produced. The damage to the ecology is self-evident.

[0011] However, since laterite nickel ore contains about 20-45wt% iron and 1-3wt% nickel at the same time, it uses a semi-purified form of pyrometallurgy to refine cobalt-containing nickel-iron alloy (common Indonesian nickel-iron plant nickel-iron contains 0.2-2wt% cobalt, 3-18wt% nickel, and 70-80wt% iron), which can recover useful metal iron and nickel as well as cobalt in the form of alloy as much as possible, and further use it as the basic material of stainless steel to produce stainless steel to obtain the maximum economic benefit. Compared with the wet extraction of nickel and cobalt, its pyrometallurgy process has the advantages of less investment, shorter construction period, less and harmless tailings, etc. However, the existing technology of pyrometallurgy process cannot separate iron, cobalt and nickel, and can only be melted together to make nickel-iron alloy, which is further brought into the manufacture of downstream steel, or the process of further making nickel ice or acid leaching of cobalt-containing nickel-iron alloy to extract cobalt is huge and unfriendly to the environment. Therefore, designing a simple, environmentally friendly and low-carbon equipment and method to enrich and separate cobalt in the cobalt-containing nickel-iron alloy after smelting laterite nickel ore is an important problem that urgently needs to be solved in the industry. Summary of the invention

[0012] The object of the present invention is to provide a method for enriching cobalt from nickel-iron alloy by using Curie temperature, so as to solve the problems raised in the above background technology.

[0013] In order to achieve the above object, the technical solution adopted by the present invention is:

[0014] A method for enriching cobalt from a nickel-iron alloy using Curie temperature comprises the following steps:

[0015] S1: melt a cobalt-containing nickel-iron alloy whose main components are: 1wt%≤Ni≤20wt%, 0.01wt%≤Co≤10wt%, 0.1wt%≤Si≤3.5wt%, 0.1wt%≤C≤4.3wt%, 60wt%≤Fe≤90wt% in a ladle, raise the temperature to 1300-1550℃ and maintain it for 0.5-3h;

[0016] S2: blowing oxygen into the nickel-iron alloy solution to oxidize the iron in the alloy to form slag, and increase the nickel content in the nickel-iron alloy to ≥20.5wt%, and the cobalt content to ≥0.05wt%;

[0017] S3: Remove the slag and add carbon to the nickel-iron alloy to ≥2.2wt%;

[0018] S4: cooling the nickel-iron alloy solution to 1000-1250° C. and maintaining the temperature for 0.5-3 hours, adding a crystal inducing agent into the ladle, and performing homogenization vibration;

[0019] S5: stirring the cobalt-containing alloy in the molten iron ladle so that the cobalt-containing alloy contacts the bottom of the ladle by convection from top to bottom, and cooling the bottom of the molten iron ladle and increasing a magnetic field outside the bottom of the ladle to adsorb cobalt crystals on the bottom of the ladle for solidification;

[0020] S6: discharging the decobalted nickel-iron alloy from the upper part of the ladle;

[0021] S7: demoulding the cobalt-rich alloy remaining in the molten iron ladle or heating and melting it into liquid to discharge the cobalt-rich alloy.

[0022] The source of the cobalt-containing nickel-iron alloy in step S1 can be a cold solid state, or can be a molten liquid alloy iron molten after smelting in a laterite nickel ore pyrometallurgical plant.

[0023] In step S4, the crystal inducing agent is a combination of one or more of permanent magnetic material, alloy steel, electrolytic cobalt, and iron powder.

[0024] The amount of the crystal inducing agent added in step S4 is 0.01%-5% of the mass fraction of the nickel-iron alloy in the ladle.

[0025] In step S4, the homogenizing vibration uses a vibrator or sound waves, so that the solid crystal-inducing agent acts as a crystal nucleus to induce cobalt segregation and crystallization.

[0026] The stirring method in step S5 can be electromagnetic stirring, or it can be stirring by passing gas into the molten iron ladle, the gas blown into the stirring gas is any one or two of nitrogen and argon, and the blowing method is a combination of one or more of top blowing, side blowing and bottom blowing.

[0027] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0028] 1) The present invention utilizes the different Curie point temperatures of various metal elements in the cobalt-containing nickel-iron alloy after pyrometallurgy of laterite nickel ore, especially the high Curie point characteristic of cobalt, and crystallizes near the Curie temperature of cobalt during the cooling and crystallization process after the nickel-iron alloy is melted. At the same time, a cobalt-philic crystallization inducer is added to induce the segregation of cobalt and magnetic adsorption, so that the cobalt in the alloy is finally enriched at the bottom of the iron ladle, thereby achieving the purpose of enriching and separating cobalt;

[0029] 2) The present invention adds a breakthrough technical point of adjusting the composition to make its crystallization temperature close to the Curie point temperature of cobalt, which makes the method more efficient, applicable to a wider range of materials, and easier to lower the crystallization temperature and improve the enrichment yield;

[0030] 3) The present invention optimizes the existing cobalt smelting process, and has the advantages of low cost, small equipment investment, energy saving and environmental protection. At the same time, it can be enriched to different cobalt contents for direct use according to the needs of downstream industries, solving the problems of difficulty, high cost and great environmental harm in the existing cobalt-containing nickel-iron alloy enrichment and separation, which greatly promotes the new energy vehicle industry and has good economic benefits and broad market prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a process flow chart of an embodiment of the present invention.

[0032] Figure 2 FIG. 4 is a graph showing the relationship between the oxidation reaction free energy and temperature according to an embodiment of the present invention. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0034] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] like Figure 1 As shown, the method of enriching cobalt from nickel-iron alloy by using Curie temperature of the present invention utilizes the different Curie temperature of each metal element in the nickel-iron alloy containing cobalt after pyrometallurgy of laterite nickel ore, especially the high Curie point characteristic of cobalt (the Curie temperature of cobalt is 1150°C, the Curie temperature of iron is 786°C, and the Curie temperature of nickel is 376°C), crystallizes near the Curie temperature of cobalt during the cooling and crystallization process after the nickel-iron alloy is melted, and at the same time, a cobalt-philic crystallization inducer is added to induce the segregation of cobalt and magnetic adsorption, so that the cobalt in the alloy is finally enriched at the bottom of the iron ladle, so as to achieve the purpose of enriching and separating cobalt. The method specifically comprises the following steps:

[0036] S1: melt the cobalt-containing nickel-iron alloy whose main components are: 1wt%≤Ni≤20wt%, 0.01wt%≤Co≤10wt%, 0.1wt%≤Si≤3.5wt%, 0.1wt%≤C≤4.3wt%, 60wt%≤Fe≤90wt% in a molten iron ladle, raise the temperature to 1300-1550℃ and keep it for 0.5-3h; the source of the cobalt-containing nickel-iron alloy can be cold solid or molten liquid alloy iron after smelting in a laterite nickel ore pyrometallurgical plant. If liquid alloy iron is used, a large amount of melting energy consumption can be saved, making the economic efficiency of this technology better after industrialization;

[0037] S2: Blow oxygen into the nickel-iron alloy solution to oxidize the iron in the alloy to form slag, and increase the nickel content in the nickel-iron alloy to ≥20.5wt%, and the cobalt content to ≥0.05wt%; the main metal elements in the cobalt-containing nickel-iron alloy are iron, cobalt, and nickel. Figure 2It can be seen from the relationship diagram between the free energy of oxidation reaction and temperature that within the temperature range of 1300-1550℃, the oxygen affinity of iron, cobalt and nickel is: Fe>Co>Ni. Therefore, when oxygen is blown into the nickel-iron alloy solution, oxygen will first react with iron to form iron oxide slag instead of reacting with nickel and cobalt, which will reduce the iron content in the solution and increase the nickel and cobalt content. Here, since the mother liquor is enriched, it will be more efficient than the CN114214526A technology. At the same time, after experiments, it was found that in order to ensure that the recovery rate of nickel and cobalt in the oxygen blowing slag making process is higher than 95%, it is more appropriate to blow the nickel content to 22-38wt%. If the nickel content is further increased to ≥38wt%, although it is beneficial to the subsequent steps of cobalt extraction, the recovery rate of nickel and cobalt will decrease. Therefore, the degree of blowing should be further determined based on the market nickel and cobalt prices. For example, if the cobalt price is higher than 500,000 / ton, the nickel blowing grade can be increased to more than 38wt%;

[0038] The oxygen blowing described in the present invention can be one of oxygen and air, or a mixture of the two in any proportion;

[0039] In the slag making process of the present invention, limestone, aluminum, silicon powder, calcium silicon wire, foam slag inhibitor, etc. can be added to control foam slag and further refine to reduce harmful components in the alloy; solid nickel iron, dust removal ash, sintered ore and scrap steel and other cold materials can also be added to reduce slag temperature overheating;

[0040] S3: Remove the slag and add carbon to the nickel-iron alloy to ≥2.2wt%; the carbon addition operation is generally completed using conventional steelmaking carburizers and carburizing methods. From the calculation formula of the crystallization temperature Ts of steel, it can be seen that the main alloying elements that affect the crystallization temperature of nickel-iron alloy are C and Ni:

[0041] Ts=1536℃-(78C%+7.6Si%+4.9Mn%+34P%+30S%+5Cu%+3.1Ni%...)

[0042] In the process of improving the nickel grade in step S2, a large amount of carbon will be oxidized, so it is necessary to increase the carbon content in step S2 to reduce the crystallization temperature of the nickel-iron alloy. At the same time, the increase in nickel content not only drives the increase in cobalt content, which is beneficial to the enrichment of subsequent steps, but also contributes to the decrease in crystallization temperature. Here, due to the carbon increase and other measures taken on the alloy liquid before cobalt enrichment, the controllable range of alloy crystallization point temperature is greatly improved compared with CN114214526A.

[0043] S4: cooling the nickel-iron alloy solution to 1000-1250°C and maintaining the temperature for 0.5-3 hours, while adding a crystal inducer into the iron ladle and performing homogenization vibration; in this step, the homogenization vibration may be performed by a vibrator or by means of sound waves, so that the solid crystal inducer acts as a crystal nucleus to induce cobalt segregation and crystallization; the crystal inducer is one or more of a permanent magnetic material, alloy steel, electrolytic cobalt, and iron powder, and the preferred crystal inducer is a permanent magnetic samarium-cobalt alloy, which is more efficient than the crystal inducer described in CN114214526A, and the amount of the crystal inducer added each time is 0.01%-5% of the mass fraction of the nickel-iron alloy in the iron ladle; the crystal inducer here is different from the inoculant in the general crystallization process, and the effect of the crystal inducer is opposite to that of the inoculant, the inoculant is to homogenize the overall metal particles, and the crystal inducer of the present invention is to induce harmful segregation of certain grains. Meanwhile, the cooling measures in this step may be natural cooling or artificial intervention such as adding a water cooling pipe to the outer wall of the ladle; maintaining the temperature at 1000-1250°C for 0.5-3 hours may be natural insulation or artificial intervention insulation such as induction heating, radiation heating, etc., wherein the 1000-1250°C mentioned here is determined by the crystallization temperature caused by the alloy composition;

[0044] S5: stirring the cobalt-containing alloy in the ladle so that the cobalt-containing alloy contacts the bottom of the ladle by convection from top to bottom, and at the same time cooling the bottom of the ladle and increasing the magnetic field outside the bottom of the ladle to adsorb the cobalt crystals on the bottom of the ladle for solidification; the stirring method can be electromagnetic stirring, or gas can be introduced into the ladle for stirring, and the gas blown into the ladle can be any one of nitrogen and argon or a mixture of the two; the blowing method can be any one of top blowing, side blowing, bottom blowing or a combination of more than one; in order to reduce the cobalt crystals segregated by electromagnetic force on the cobalt-containing alloy and solidify on the ladle wall, the present invention preferably uses gas stirring;

[0045] S6: discharging the decobalted nickel-iron alloy from the upper part of the ladle;

[0046] S7: demoulding the cobalt-rich alloy remaining in the molten iron ladle or heating and melting it into liquid to discharge the cobalt-rich alloy.

[0047] The ladle described in the above-mentioned steps S1-S3 and the ladle described in the steps S4-S7 can complete all the steps described in S1-S7 in the same ladle according to the process temperature requirements, or can complete the steps S1-S3 and S4-S7 in two different ladles respectively; the ladle described in the steps S1-S3 is a ladle with a steel shell inner layer built with refractory materials, and the ladle described in the steps S4-S7 can be a ladle with a steel shell inner layer built with refractory materials, or can be a ladle of high-temperature alloy without built with refractory materials.

[0048] The steps S4-S5 can be repeated to gradually increase the yield of cobalt. At the same time, the present invention can also be used to process materials whose main metal element content meets the requirements of step S1, such as ternary battery waste and alloy waste.

[0049] The specific embodiments of the present invention are as follows:

[0050] Example 1

[0051] S1: A nickel iron factory adopts the rotary kiln + ore-fired furnace RKEF process technology to smelt high-nickel and low-iron laterite nickel ore. The cobalt-containing nickel iron product produced by the factory mainly contains 0.3wt% cobalt, 12wt% nickel, 80wt% iron, 2.8wt% carbon, and the rest are other impurities; the raw materials are put into the molten iron ladle of the present invention in liquid form, and the cobalt is enriched by the method shown in the present invention; the temperature of the raw materials put into the separation bag of the nickel iron factory is about 1390°C, and about 6 tons of alloy water are put in at one time; after calculation, the crystallization temperature of the alloy of this component is about 1260°C; the raw material temperature is much higher than the crystallization temperature, and no heating and melting is required, and the raw materials directly enter the S2 step for refining and slag making;

[0052] S2: After blowing air into the slag, the slag is removed, and the main components after refining are determined to contain 0.58wt% cobalt, 25wt% nickel, 0.8wt% carbon, and the rest are iron and other impurities. It is calculated that the crystallization temperature of this alloy is 1380°C, which cannot meet the requirements of the present invention and needs to be supplemented with carbon; the carbon is supplemented to 3.8wt%, and it is calculated that the crystallization temperature of the alloy is 1145°C at this time;

[0053] S3: The alloy in step S2 is cooled and maintained at 1120°C-1200°C, and the temperature is repeatedly raised and lowered within this temperature range within 2 hours, while 0.3 kg of samarium cobalt alloy (SmCo5) with a particle size of about 1 mm, 1 kg of electrolytic cobalt with a particle size of about 1 mm, and 3 kg of iron powder with a particle size of 2 mm are slowly and intermittently added, and a vibrator is installed on the outer wall of the ladle for intermittent vibration;

[0054] S4: A 120MT electromagnet is set outside the bottom of the ladle, and argon is blown into the top of the ladle intermittently for stirring. Each blowing time is 20-30 seconds, and the pause time is 3-5 minutes;

[0055] S5: repeat steps S3 and S4 twice, lower the temperature of the molten iron in the ladle to 1150°C and keep it still for 0.5 hours, pour out the unsolidified liquid alloy on the top, and the measured weight is 5.8 tons, containing 0.1wt% cobalt;

[0056] S6: The alloy solidified at the bottom was heated by induction heating and poured out. The measured weight was 0.1 ton, containing 15.1wt% cobalt.

[0057] In summary, except for the loss caused by the ladle sticking to the ladle wall and casting, although the cobalt content in the bottom liquid is only 12.1wt%, after deducting the influence of the addition of the crystal inducer and the loss, the comprehensive recovery rate of the cobalt-rich alloy at the bottom is 61.5%. This cobalt-enriched alloy can be further used as a high-temperature alloy material, or enter the wet process to reduce acid consumption and tailings pollution.

[0058] Example 2

[0059] S1: A nickel iron factory adopts RKEF process technology to smelt high-cobalt and low-nickel laterite nickel ore. The main components of the cobalt-containing nickel iron product produced by it are: 0.65wt% cobalt, 10wt% nickel, 80wt% iron, 2.2wt% carbon, and the rest are other impurities; it is put into the molten iron ladle described in the present invention in liquid form, and the cobalt is enriched by the method shown in the present invention; the temperature of the incoming materials put into the separation bag of the nickel iron factory is about 1380℃, and about 30 tons of alloy water are put in at a time as mother liquor. After calculation, the crystallization temperature of this component alloy is about 1310℃; the incoming material temperature is much higher than the crystallization temperature, and there is no need to heat and melt, and it directly enters the S2 step for refining and slag making;

[0060] S2: After blowing oxygen-enriched air with an oxygen content of 26% into the slag, the slag was removed, and the main components after refining were determined to contain 1.6wt% cobalt, 26wt% nickel, 0.5wt% carbon, and the rest were iron and other impurities. It was calculated that the crystallization temperature of the alloy was about 1398°C, which could not meet the requirements of the present invention and needed to be supplemented with carbon; the carbon was supplemented to 3.9wt%, and it was calculated that the crystallization temperature of the alloy was about 1128°C at this time;

[0061] S3: The alloy in step S2 is cooled and maintained at 1100°C-1200°C, and the temperature is repeatedly raised and lowered within this temperature range within 3 hours, while 0.2kg of samarium cobalt alloy (SmCo5) with a particle size of about 1mm, 10kg of ferrite magnet powder with a particle size of about 1mm, and 20kg of 0Cr13 steel with a particle size of 2mm are slowly and intermittently added, and ultrasonic vibration is set on the top, and intermittent vibration is performed;

[0062] S4: A 150MT electromagnet is set outside the bottom of the ladle, and argon is blown into the top of the ladle intermittently for stirring. Each blowing time is 30-50 seconds, and the rest time is 5-10 minutes;

[0063] S5: repeat steps S3 and S4 three times, lower the temperature of the molten iron in the ladle to 1130°C and keep it still for 1 hour, pour out the unsolidified liquid alloy on the top, and the measured weight is 28.9 tons, containing 0.16wt% cobalt;

[0064] S6: The alloy solidified at the bottom was heated by induction heating and poured out. The measured weight was 0.7 tons, containing 20.97wt% cobalt.

[0065] In summary, except for the loss caused by the ladle sticking to the ladle wall and casting, although the cobalt content in the bottom liquid is only 20.97wt%, the cobalt content in the cobalt-rich alloy at the bottom is comparable to that in the mother liquor, and the comprehensive recovery rate is 74.75%. This cobalt-enriched alloy can be further used as an alloy material, or enter the wet process to extract cobalt, which can reduce acid consumption and tailings pollution.

[0066] The cobalt-rich alloy can also be reused in a ladle with a capacity of about 1 ton and processed and purified again using the method shown in the present invention, or the cobalt-rich alloys from multiple ladles of iron described in this example can be added to a larger ladle and further enriched and purified using the method shown in the present invention until the cost of this method is higher than the value of the cobalt-rich alloy next time.

[0067] Example 3

[0068] S1: A factory purchased a batch of cobalt-containing nickel beans, which are solid particles at room temperature. After testing, the main components are: 1.65wt% cobalt, 26wt% nickel, 67wt% iron, 1.2wt% carbon, and the rest are other impurities; the method described in the present invention is used to enrich cobalt; after calculation, the crystallization temperature of this component alloy is about 1330°C;

[0069] S2: First, 10 tons of nickel beans are added into the medium frequency furnace, heated to 1460℃ for melting and maintained for 0.5h, and carbon is added to 4.3wt%, and then the alloy molten iron is poured into the ladle to be treated. According to calculation, the crystallization temperature of the alloy is about 1096℃ at this time;

[0070] S3: The alloy in step S2 is cooled and maintained at 1080°C-1130°C, and the temperature is repeatedly raised and lowered within this temperature range within 2.5 hours, while slowly and intermittently adding samarium cobalt alloy (Sm2Co 17 )0.1kg, 10kg ferrite magnet powder with a particle size of about 1mm, 20kg 45# steel with a particle size of 2mm, ultrasonic vibration and intermittent vibration are set on the top;

[0071] S4: A 150MT electromagnet is set outside the bottom of the ladle, and argon is blown into the top of the ladle intermittently for stirring. Each blowing time is 30-50 seconds, and the rest time is 5-8 minutes;

[0072] S5: repeat steps S3 and S4 five times, lower the temperature of the molten iron in the ladle to 1100°C and keep it still for 0.5 hours, pour out the unsolidified liquid alloy on the top, and the measured weight is 9 tons, containing 0.12wt% cobalt;

[0073] S6: The alloy solidified at the bottom was poured out by induction heating. The measured weight was 0.79 tons and contained 18.43wt% cobalt.

[0074] In summary, except for the loss caused by the ladle sticking to the ladle wall and casting, the comprehensive recovery rate of cobalt in the cobalt-rich alloy at the bottom is 87.6%. The cobalt-enriched alloy can be further used as alloy material, battery material, or enter the wet process to extract cobalt, which can reduce acid consumption and tailings pollution.

[0075] The cobalt-rich alloy can also be processed and purified again using a ladle with a capacity of about 1 ton using the method shown in the present invention until the cost of this method is higher than the value of the cobalt-rich alloy next time.

[0076] Example 4

[0077] S1: A factory purchased a batch of nickel-cobalt alloy, which was in solid block at room temperature. After analysis, the main components were: 15wt% cobalt, 70wt% nickel, 17wt% iron, 0.1wt% carbon, and the rest were other impurities. The method described in the present invention was used to enrich cobalt. After calculation, the crystallization temperature of this component alloy was about 1260°C.

[0078] S2: First, 5 tons of nickel-cobalt alloy is added into the medium frequency furnace, heated to 1380℃ for melting and maintained for 3h, and carbon is added to 2.2wt%, and then the alloy molten iron is poured into the ladle to be treated. According to calculation, the crystallization temperature of the alloy is about 1098℃ at this time;

[0079] S3: The alloy in step S2 is cooled and maintained at 1080℃-1130℃, and the temperature is repeatedly raised and lowered within this temperature range within 2 hours, while Sm2Co alloy (Sm2Co 17 ) 1kg, 20kg of pure iron powder with a particle size of about 2mm, ultrasonic vibration is set on the top, and intermittent vibration;

[0080] S4: A 150MT electromagnet is set outside the bottom of the ladle, and argon is blown into the top of the ladle intermittently for stirring. Each blowing time is 20-35 seconds, and the rest time is 5-6 minutes;

[0081] S5: repeat steps S3 and S4 five times, lower the temperature of the molten iron in the ladle to 1100°C and keep it still for 1 hour, pour out the unsolidified liquid alloy on the top, and the measured weight is 3.6 tons, containing 3.89wt% cobalt;

[0082] S6: The alloy solidified at the bottom was heated by induction heating and poured out. The measured weight was 1.30 tons, containing 46wt% cobalt.

[0083] In summary, except for the loss caused by the ladle sticking to the ladle wall and casting, the comprehensive recovery rate of cobalt in the cobalt-rich alloy at the bottom is 79.6%. The cobalt-enriched alloy can be further used as alloy material, battery material, or enter the wet process to extract cobalt, which can reduce acid consumption and tailings pollution.

[0084] The upper alloy containing 3.89 wt% cobalt in this embodiment can be treated again using the method shown in the present invention until the treatment cost is higher than the product selling price and loses its economic value.

[0085] At the same time, the bottom alloy containing 46wt% cobalt in this embodiment can be processed and purified again using the method shown in the present invention until the cost of this method is higher than the value of the next cobalt-rich alloy; the bottom alloy containing 46wt% cobalt in this embodiment can also be directly used on the cobalt-based alloy base material; the bottom alloy containing 46wt% cobalt in this embodiment and the further enriched cobalt-containing alloy can also be made into particles by water quenching or air quenching, and then sent to the downstream wet process to produce cobalt sulfate or electrolytic cobalt.

[0086] According to public data, the world's production capacity of nickel-iron alloys smelted from laterite nickel ore (mainly concentrated in China and Indonesia) is about 22 million tons in 2021. If calculated based on an average cobalt content of 0.3wt% in the alloy, more than 66,000 tons of metallic cobalt will be wasted each year from cobalt-containing alloys smelted from laterite nickel ore (the global production of metallic cobalt in 2021 is about 170,000 tons). Calculated based on the average cobalt price of 363,000 yuan / ton in 2021, it is estimated that the value of cobalt lost from alloys smelted from laterite nickel ore in 2023 will be about 23.958 billion yuan, and this part of cobalt is a harmful component in downstream stainless steel; the present invention turns harm into treasure, optimizes the purity of downstream steel, and also obtains valuable cobalt resources. The present invention is only an enrichment method. There are inevitably mixed crystals at the crystallization interface, and it cannot be completely purified into cobalt metal, but it has low cost, small equipment investment, and can be enriched to different cobalt contents for direct use according to the needs of downstream industries. For example, the bottom alloy enriched to contain about 20-60wt% cobalt can be directly used in the cobalt-based alloy base material, while saving the material costs of the associated nickel and iron; the bottom alloy enriched to contain more than 10wt% cobalt and the further enriched cobalt-containing alloy can also be made into particles by water quenching or air quenching methods, and then used for the downstream wet process to produce cobalt sulfate or electrolytic cobalt. A deep understanding of the raw material composition and downstream demand can be used to formulate an economically reasonable enrichment content and process flow, which will make the present invention more flexible and more competitive in the market.

Claims

1. A method for enriching cobalt from nickel-iron alloy using Curie temperature, characterized in that: The following steps are involved: S1: melt a cobalt-containing nickel-iron alloy whose main components are: 1wt%≤Ni≤20wt%, 0.01wt%≤Co≤10wt%, 0.1wt%≤Si≤3.5wt%, 0.1wt%≤C≤4.3wt%, 67wt%≤Fe≤90wt% in a ladle, raise the temperature to 1300-1550℃ and keep it for 0.5-3h; S2: blowing oxygen into the nickel-iron alloy solution to oxidize the iron in the alloy to form slag, and increase the nickel content in the nickel-iron alloy to ≥20.5wt%, and the cobalt content to ≥0.05wt%; S3: Remove the slag and add carbon to the nickel-iron alloy to ≥2.2wt%; S4: cooling the nickel-iron alloy solution to 1000-1250° C. and maintaining the temperature for 0.5-3 hours, adding a crystal inducing agent into the ladle, and performing homogenization vibration; S5: stirring the cobalt-containing alloy in the molten iron ladle so that the cobalt-containing alloy contacts the bottom of the ladle by convection from top to bottom, and cooling the bottom of the molten iron ladle and increasing a magnetic field outside the bottom of the ladle to adsorb cobalt crystals on the bottom of the ladle for solidification; S6: discharging the decobalted nickel-iron alloy from the upper part of the ladle; S7: demoulding or heating and melting the cobalt-rich alloy remaining in the ladle into a liquid state to discharge the cobalt-rich alloy; The amount of the crystal inducing agent added in step S4 is 0.01%-5% of the mass fraction of the nickel-iron alloy in the ladle; In step S4, the homogenization vibration is performed by using a vibrator, so that the solid crystal inducing agent acts as a crystal nucleus to induce cobalt segregation and crystallization; The stirring method in step S5 can be electromagnetic stirring, or it can be stirring by passing gas into the molten iron ladle, the gas blown into the stirring gas is any one or two of nitrogen and argon, and the blowing method is a combination of one or more of top blowing, side blowing and bottom blowing.

2. A method for enriching cobalt from a nickel-iron alloy using Curie temperature according to claim 1, characterized in that: The source of the cobalt-containing nickel-iron alloy in step S1 can be a cold solid state, or can be a molten liquid alloy iron molten after smelting in a laterite nickel ore pyrometallurgical plant.

3. A method for enriching cobalt from a nickel-iron alloy using Curie temperature according to claim 1, characterized in that: In step S4, the crystal inducing agent is a combination of one or more of permanent magnetic material, electrolytic cobalt, and iron powder.